Heating control method for reducing decarburization of second-fire high-temperature gear steel

By optimizing the heating process and production schedule, the problem of excessive thickness of the decarbonization layer of the second fire high-temperature gear steel is solved, and the effect of reducing the thickness of the decarbonization layer and improving the material yield is achieved, saving the cost of repairing and grinding.

CN119056865AInactive Publication Date: 2024-12-03NANJING IRON & STEEL CO LTD

Patent Information

Application Number
CN202411134321.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the prior art During the steel rolling process, the thickness of the decarbonized layer of the second fire high-temperature gear steel cannot meet customer requirements, resulting in increased repair costs and reduced material yield.

Method used

By optimizing the heating process and production schedule, including controlling the preheating and heating temperature sections, high temperature period time limit, specific steel types are prohibited from being produced together, and empty steps in the furnace and water tanks along the line are removed during rolling.

Benefits of technology

The thickness of the decarbonized layer on the surface of the gear steel is effectively reduced to 0.5-0.6D%, improving the yield and saving grinding costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004998918320000021
    Figure BDA0004998918320000021
Patent Text Reader

Abstract

The invention discloses a heating control method for reducing decarburization of second-fire high-temperature gear steel. The heating control method comprises the following steps: 1) optimizing a production scheduling plan; 2) optimizing a heating process; (3) when high-temperature gear steel billets are fed into the furnace, one gear steel billet is loaded in one step; (4) the time of a high-temperature section is less than 80 minutes; and (5) all the water tanks along the line fall off during rolling. By optimizing the heating process, the thickness of the decarburized layer on the surface of the steel for the second-fire high-temperature gear is reduced, and the coping cost of the steel billet for the second-fire high-temperature gear is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of steel rolling, and in particular to a heating control method for reducing decarburization of double-fire high-temperature gear steel. Background Art

[0002] With the development of aviation, mechanical and automotive fields, the requirements for transmission gears are getting higher and higher. Gears, as transmission equipment, must withstand heavy loads, cyclic stresses and large impact stresses during service. Therefore, the surface quality and performance requirements for gear steel are also getting higher and higher. Many customers require that gear steel be smelted in an electric furnace, and then subjected to two-stage rolling after blanking. The thickness of the decarburized layer of the finished product after rolling is less than 0.8D% (D round steel diameter). The heating time of the blank is about 8 to 10 hours when blanking. The surface decarburization of the blank is thicker after blanking. During rolling, high-temperature rolling is performed to meet the grain size requirements, resulting in the decarburization of the finished product unable to meet the delivery requirement of less than 0.8D%. In order to meet the delivery requirements, the blank is peeled and then rolled, which not only increases the grinding cost, but also reduces the yield rate by more than 2%.

[0003] Therefore, it is necessary to develop a new heating control method to reduce the thickness of the decarburized layer on the surface of the rod. Summary of the invention

[0004] Purpose of the invention: In view of the shortcomings and defects of the prior art, the present invention provides a heating control method for reducing decarburization of double-fire high-temperature gear steel. By optimizing the heating process, the thickness of the decarburization layer on the surface of double-fire high-temperature gear steel is reduced, and the grinding cost of double-fire high-temperature gear steel billets is reduced.

[0005] Technical solution: A heating control method for reducing decarburization of a double-fire high-temperature gear steel of the present invention is characterized by comprising the following steps:

[0006] 1) Optimize production scheduling;

[0007] 2) Optimize heating process;

[0008] 3) When high-temperature gear steel billets are put into the furnace, one empty step is installed;

[0009] 4) The high temperature period is less than 80 minutes;

[0010] 5) All water tanks along the line are lowered during rolling.

[0011] Among them, in the step 1), the cold shear steel is arranged in front of the high-temperature gear steel and is prohibited from being arranged together with the high-temperature section steel that needs to be warmed up.

[0012] Among them, the steel types that need to be kept warm in the high temperature section include bearing steel and free-cutting steel.

[0013] Wherein, in the step 2), the temperatures of the preheating section, the first heating section, the second heating section, the first soaking section, the second soaking section, the P1 temperature and the P6 sizing temperature are controlled.

[0014] Wherein, in the step 2), the temperature of the preheating section is controlled to be ≤800°C, the temperature of the first heating section is ≤950°C, the temperature of the second heating section is 1050°C to 1120°C, the temperature of the first soaking section is 1060°C to 1140°C, the temperature of the second soaking section is 1080°C to 1140°C, the temperature of P1 is 950°C to 1080°C, and the temperature of P6 entering the sizing section is ≥930°C.

[0015] Preferably, the second heating stage temperature is 1080°C.

[0016] Preferably, the temperature of the soaking stage is 1120°C.

[0017] Preferably, the temperature of the second soaking stage is 1110°C.

[0018] Preferably, the P1 temperature is 1020°C.

[0019] Preferably, in step 4), the high temperature section includes a first soaking section and a second soaking section.

[0020] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: By optimizing the heating process, the idle step in the furnace and the production schedule, the surface decarburization is reduced to 0.5-0.6D%, which not only meets the delivery requirements, but also increases the yield rate by more than 2.4%, and saves the cost of billet grinding. DETAILED DESCRIPTION

[0021] The technical solution of the present invention is further described below in conjunction with specific implementation methods.

[0022] A heating control method for reducing decarburization of a double-fire high-temperature gear steel according to the present invention comprises the following steps:

[0023] 1) Optimize production scheduling; cold shear steel should be prioritized before high-temperature gear steel, and it is prohibited to arrange it together with high-temperature steels such as bearing steel and free-cutting steel that need to be warmed up.

[0024] 2) Optimize the heating process; control the preheating section temperature ≤ 800°C, the heating section temperature ≤ 950°C, the heating section temperature 1050°C to 1120°C (preferably 1080°C), the soaking section temperature 1060°C to 1140°C (preferably 1120°C), the soaking section temperature 1080°C to 1140°C (preferably 1110°C), the P1 temperature 950°C to 1080°C (preferably 1020°C), and the P6 sizing temperature ≥ 930°C.

[0025]

[0026] 3) When high-temperature gear steel billets are put into the furnace, one empty step should be installed.

[0027] 4) The high temperature section time is less than 80 minutes; the high temperature section includes the first and second soaking sections.

[0028] 5) All water tanks along the line are lowered during rolling.

[0029] After testing, it was found that by optimizing the heating process, furnace idle steps and production scheduling, the surface decarburization of the gear steel was reduced to 0.5-0.6D%, which not only met the delivery requirements, increased the yield rate by 2.4%, but also saved the billet grinding cost of 136.5 yuan / ton.

Claims

1. A heating control method for reducing decarburization of high-temperature gear steel in two-fire, Features: The steps include: 1) Optimize production scheduling; 2) Optimize heating process; 3) When high-temperature gear steel billets are put into the furnace, one empty step is installed; 4) The high temperature period is less than 80 minutes; 5) All water tanks along the line are lowered during rolling.

2. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 1, Features: In the step 1), the cold shear steel is arranged in front of the high-temperature gear steel and is prohibited from being arranged together with the high-temperature section steel that needs to be warmed up.

3. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 2, Features: The steel types that need to be kept warm in the high temperature section include bearing steel and free-cutting steel.

4. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 1, Features: In the step 2), the temperatures of the preheating section, the first heating section, the second heating section, the first soaking section, the second soaking section, the P1 temperature and the P6 sizing temperature are controlled.

5. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 4, Features: In the step 2), the temperature of the preheating section is controlled to be ≤800°C, the temperature of the first heating section is ≤950°C, the temperature of the second heating section is 1050°C to 1120°C, the temperature of the first soaking section is 1060°C to 1140°C, the temperature of the second soaking section is 1080°C to 1140°C, the temperature of P1 is 950°C to 1080°C, and the temperature of P6 for sizing is ≥930°C.

6. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 5, Features: The temperature of the second heating stage is 1080°C.

7. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 5, Features: The temperature of the soaking stage is 1120°C.

8. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 5, Features: The temperature of the second soaking stage is 1110°C.

9. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 5, Features: The P1 temperature is 1020°C.

10. The heating control method for reducing decarburization of double-fire high-temperature gear steel according to claim 1, Features: In the step 4), the high temperature section includes a first and a second soaking section.

Citation Information

Patent Citations

  • Method for eliminating cracks in steel surface of cold-rolled saw web

    CN107299201A

  • Heating method for decreasing depth of hub bearing steel decarburized layer

    CN107513606A

  • Production method of spring steel wire for automotive suspension

    CN116550750A

  • Heating control method for reducing decarburization of steel for guide rail

    CN117265250A

  • Method for reducing thickness of decarburized layer of bar spring steel

    CN117286315A

Cited By

  • Hot rolling method for improving surface decarburization of gear steel

    CN122517366A