Cast iron roller manufacturing method and casting tool
By designing a special sand box structure and casting path in the cast iron roll manufacturing method, impurities in the molten iron are brought to the top of the roll, solving the problem of many slag and air holes in the roll in the prior art, and improving the compactness of the roll and performance.
Patent Information
- Application Number
- CN202411200915.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-12-03
AI Technical Summary
In the existing cast iron roll manufacturing method, due to the impurities in the cast iron, there are many slags and pores inside the roll, and the overall tightness is not high.
A cast iron roll manufacturing method is designed, by shaping and combining the riser sand box, gate sand box, straight gate sand box, lower roller neck sand box and base sand box, and when pouring the molten iron, the molten iron first. The runner of the straight gate sand box flows into the runner of the base sand box, and then flows in a horizontal or inclined direction, spiral up to the cavity, driving impurities to the top, reducing slag and air holes inside the roll.
It effectively improves the overall tightness of the roll, reduces internal slag inclusions and pores, and improves the wear resistance and thermal crack resistance of the roll.
Smart Images

Figure CN119057034A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of roller casting, and in particular to a method for manufacturing a cast iron roller and a casting tool. Background Art
[0002] The casting method of infinitely chilled cast iron rolls is a manufacturing method that uses a cold mold (made of gray cast iron) to produce a chilling reaction with molten iron on the roll body, so that the roll surface reaches a white cast iron structure with an ideal hardness. The molten iron is poured into the cold mold, and the cast iron surface in contact with the cold mold forms a certain thickness of white cast iron structure due to the rapid cooling rate. The hardness of this structure is relatively high, while the deep part away from the cold mold forms a gray cast iron structure due to the slow cooling rate. The rolls cast in this way have good wear resistance, thermal cracking resistance and spalling resistance, so they are widely used in rolling mills in steel plants.
[0003] At present, in the process of pouring molten iron into the cold mold, since the molten iron after pouring contains impurities such as molten iron slag, the final roller is formed with slag inclusions inside, many pores, and the overall compactness of the roller is not high. Summary of the invention
[0004] The purpose of the present application includes, for example, providing a method for manufacturing a cast iron roll, which can improve the overall compactness of the roll.
[0005] The purpose of the present application also includes providing a casting tool that can improve the overall compactness of the rolling mill.
[0006] The embodiments of the present application can be implemented as follows:
[0007] An embodiment of the present application provides a method for manufacturing a cast iron roll, the manufacturing method comprising:
[0008] Molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask;
[0009] heating the cold type;
[0010] Combining the riser flask, the gate flask, the sprue flask, the cold mold, the lower roll neck flask and the base flask;
[0011] Detecting the temperature of the cold type;
[0012] When the temperature of the cold mold is within a preset temperature range, molten iron is poured into the pouring port of the pouring flask, so that the molten iron first flows from the runner of the sprue flask into the runner of the base flask from top to bottom, then flows in the runner of the base flask, and finally spirally rises in the base flask, the lower roll neck flask, the cold mold and the riser flask until the mold cavity is filled.
[0013] Optionally, in the step of pouring molten iron into the pouring port of the pouring flask, the pouring time of the molten iron is 40-50 seconds;
[0014] When the molten iron is poured to 3 / 4 of the preset riser height, point pouring is performed until the molten iron is poured to the preset riser height.
[0015] Optionally, after the step of pouring molten iron into the pouring port of the pouring flask, the method further comprises:
[0016] Cover the riser with insulation to prevent the riser from shrinking.
[0017] Optionally, after the step of covering the riser with a heat-insulating agent, the method further comprises:
[0018] Unboxing is performed after a preset time;
[0019] Cleaning the riser sand box, the gate sand box, the sprue sand box, the lower roll neck sand box and the base sand box;
[0020] The resin sand cleared out of the riser sand box, the gate sand box, the sprue sand box, the lower roll neck sand box and the base sand box is recovered.
[0021] Optionally, before the step of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask, the step further includes:
[0022] The molding sand, furan resin and benzenesulfonic acid curing agent are mixed in proportion by using a sand mixer to form resin sand.
[0023] Optionally, the step of heating the cold type includes:
[0024] Place the cold mold in a box-type resistance furnace and heat it to 140-160°C and keep the temperature constant;
[0025] A coating is applied inside the cold mold and maintained at a constant temperature, wherein the coating comprises coke powder, graphite powder and syrup, and the ratio of the coke powder, the graphite powder and the syrup is 5:3:2.
[0026] Optionally, the step of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask comprises:
[0027] The lower roll neck flask is molded:
[0028] Insert the lower roll neck model into the lower roll neck sand box, and make the outer circle stop of the lower roll neck model butt with the inner circle stop of the molding plate;
[0029] Injecting resin sand into the lower roll neck sand box by using a sand mixer;
[0030] The resin sand in the lower roll neck sand box is vibrated and compacted by a vibrator.
[0031] Optionally, after the step of molding the lower roll neck flask, the method further includes:
[0032] Modeling the base sand box:
[0033] The base flask is arranged on the lower roll neck flask;
[0034] Pre-embedding a runner white mold in the base sand box so that the runner white mold is tangent to the outer circle of the lower roll neck model;
[0035] Injecting resin sand into the base sand box using a sand mixer;
[0036] The resin sand in the base sand box is vibrated and compacted by using a vibrator.
[0037] Optionally, the step of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask comprises:
[0038] The riser sand box is molded:
[0039] Inserting the upper roll neck model into the riser sand box, and making the outer circle stop of the upper roll neck model butt with the inner circle stop of the molding plate;
[0040] Injecting resin sand into the riser sand box using a sand mixer;
[0041] The resin sand in the riser sand box is vibrated and compacted by using a vibrator.
[0042] Optionally, the step of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask comprises:
[0043] The sprue sand box is molded:
[0044] Placing the sprue sand box horizontally on the molding site;
[0045] Arranging a sprue white mold in the sprue sand box;
[0046] Injecting resin sand into the sprue sand box using a sand mixer;
[0047] The resin sand in the sprue sand box is vibrated and compacted by using a vibrator.
[0048] Optionally, the step of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask comprises:
[0049] The gate sand box is molded:
[0050] Placing the pouring sand box on a molding site;
[0051] Arranging a gate model in the gate sand box;
[0052] Injecting resin sand into the pouring sand box using a sand mixer;
[0053] The resin sand in the pouring sand box is vibrated and compacted by using a vibrator.
[0054] Optionally, the step of combining the riser flask, the gate flask, the sprue flask, the cold mold, the lower roll neck flask and the base flask comprises:
[0055] The base sand box, the cold mold, the riser sand box, the sprue sand box, and the gate sand box are stacked and assembled in sequence in the casting pit;
[0056] Fixing the sprue sand box and the base sand box with bolts;
[0057] The gate sand box and the sprue sand box are fixed with bolts.
[0058] Optionally, before the step of pouring molten iron into the pouring port of the pouring flask, the method further comprises:
[0059] Melting molten iron in a medium frequency furnace;
[0060] Pour molten iron into a ladle;
[0061] Use a crane to lift the molten iron ladle to the top of the casting pit.
[0062] The present application also provides a casting tool, including a riser sand box, a pouring gate sand box, a straight gate sand box, a cold mold, a lower roller neck sand box and a base sand box, the lower roller neck sand box and the straight gate sand box are both arranged on the top of the base sand box, and the lower roller neck sand box is located on one side of the straight gate sand box in the horizontal direction, the cold mold is arranged on the top of the lower roller neck sand box, the riser sand box is arranged on the top of the cold mold, the pouring gate sand box is arranged on the top of the straight gate sand box, a pouring gate is arranged in the pouring gate sand box, and the straight gate sand box and the base sand box are arranged with connected runners, and the base sand box, the lower roller neck sand box and the riser sand box are connected to form a mold cavity.
[0063] Optionally, a temperature measuring hole is opened on the side of the cold mold, grooves are arranged on the top and bottom surfaces of the cold mold, protrusions are arranged on the top surface of the lower roller neck sand box and the bottom surface of the riser sand box, the groove on the top surface of the cold mold cooperates with the protrusion on the bottom surface of the riser sand box, and the groove on the bottom surface of the cold mold cooperates with the protrusion on the top surface of the lower roller neck sand box, so as to ensure the concentricity between the riser sand box, the cold mold and the lower roller neck sand box.
[0064] The beneficial effects of the cast iron roll manufacturing method and casting tooling provided in the embodiments of the present application include, for example: in order to improve the overall compactness of the roll, a cast iron roll manufacturing method is designed, in which the riser flask, the pouring flask, the sprue flask, the lower roll neck flask and the base flask are first molded, and then the cold mold is heated, and then the riser flask, the pouring flask, the sprue flask, the cold mold, the lower roll neck flask and the base flask are combined, and then the temperature of the cold mold is detected. When the temperature of the cold mold is within a preset temperature range, molten iron is poured into the pouring port of the pouring flask so that the molten iron first flows from top to bottom. The runner of the sprue flask flows into the runner of the base flask, then flows in the runner of the base flask in a horizontal or inclined direction, and finally spirals up in the base flask, lower roll neck flask, cold mold and riser flask until the cavity is filled. Since the molten iron flows rapidly in the base flask in a horizontal or inclined direction, and then spirals up in the base flask, lower roll neck flask, cold mold and riser flask, in this process, impurities such as molten iron slag in the molten iron are brought to the top riser, and impurities such as molten iron slag are all located at the top of the forming roll. The part of the roll other than the top has less slag inclusions and fewer pores, thereby improving the overall compactness of the roll. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0066] Figure 1 This is a schematic diagram of the structure of the casting tool in the embodiment of the present application;
[0067] Figure 2 A cross-sectional view of a casting tool in an embodiment of the present application;
[0068] Figure 3 A schematic diagram showing a first molten iron flow path in an embodiment of the present application;
[0069] Figure 4 A schematic diagram showing a second molten iron flow path in an embodiment of the present application;
[0070] Figure 5 This is a schematic diagram of the cold type structure in the embodiment of the present application;
[0071] Figure 6 This is a flow chart of steps S1-S9 in the manufacturing method in the embodiment of the present application;
[0072] Figure 7 A schematic diagram showing the matching relationship between the lower roll neck flask, the lower roll neck model and the molding plate in the embodiment of the present application;
[0073] Figure 8 A schematic diagram showing the matching relationship between the lower roll neck flask and the base flask in the embodiment of the present application;
[0074] Fig. 9 It is a schematic diagram showing the matching relationship between the riser sand box, the upper roll neck model and the molding plate in the embodiment of the present application.
[0075] Icons: 100-riser sand box; 110-upper roll neck model; 200-gate sand box; 210-pouring gate; 300-straight gate sand box; 310-sand box body; 320-cover plate; 330-connecting assembly; 331-T-shaped pull plate; 332-oblique wedge; 400-cold mold; 410-temperature measuring hole; 500-lower roll neck sand box; 510-lower roll neck model; 600-base sand box; 610-temporary molding sealing steel plate; 620-support square box; 700-U-shaped pallet; 800-molding plate; 900-roller. DETAILED DESCRIPTION
[0076] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.
[0077] Therefore, the following detailed description of the embodiments of the present application provided in the accompanying drawings is not intended to limit the scope of the present application for which protection is sought, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0078] It should be noted that similar reference numerals and letters denote similar items in the following drawings, and therefore, once an item is defined in one drawing, further definition and explanation thereof is not required in subsequent drawings.
[0079] In the description of the present application, it should be noted that if the terms "upper", "lower", "inside", "outside", etc. appear to indicate an orientation or position relationship, it is based on the orientation or position relationship shown in the drawings, or is the orientation or position relationship in which the product of the invention is usually placed when used. It is only for the convenience of describing the present application and simplifying the description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.
[0080] In addition, the terms “first”, “second”, etc., if used, are merely used to distinguish between the descriptions and should not be understood as indicating or implying relative importance.
[0081] It should be noted that, in the absence of conflict, the features in the embodiments of the present application may be combined with each other.
[0082] See also Figure 1-Figure 5 The embodiment of the present application provides a casting tool, including a riser flask 100, a sprue flask 200, a straight sprue flask 300, a cold mold 400, a lower roll neck flask 500 and a base flask 600. The lower roll neck flask 500 and the straight sprue flask 300 are both arranged on the top of the base flask 600, and the lower roll neck flask 500 is located on one side of the straight sprue flask 300 in the horizontal direction. The cold mold 400 is arranged on the top of the lower roll neck flask 500, the riser flask 100 is arranged on the top of the cold mold 400, the sprue flask 200 is arranged on the top of the straight sprue flask 300, a pouring gate 210 is arranged in the sprue flask 200, and the straight sprue flask 300 and the base flask 600 are provided with connected flow channels, and the base flask 600, the lower roll neck flask 500 and the riser flask 100 are connected to form a cavity.
[0083] It should be pointed out that both the sprue sand box 300 and the base sand box 600 are filled with white molds. When pouring molten iron into the sprue sand box 200, the molten iron flows into the sprue sand box 300 through the pouring port 210, and the white molds in the sprue sand box 300 and the base sand box 600 are melted in turn, and connected flow channels are formed in the sprue sand box 300 and the base sand box 600, and the flow channels in the base sand box 600 are connected to the cavity. The flow channels in the base sand box 600 extend horizontally or obliquely downward, and the cavity is used to form the blank of the rolling roller 900.
[0084] A temperature measuring hole 410 is provided on the side of the cold mold 400, and a thermometer is inserted into the temperature measuring hole 410 for measuring temperature; grooves are provided on the top and bottom surfaces of the cold mold 400, and protrusions are provided on the top surface of the lower roll neck flask 500 and the bottom surface of the riser flask 100. The groove on the top surface of the cold mold 400 cooperates with the protrusion on the bottom surface of the riser flask 100, and the groove on the bottom surface of the cold mold 400 cooperates with the protrusion on the top surface of the lower roll neck flask 500 to ensure the centering between the riser flask 100, the cold mold 400 and the lower roll neck flask 500.
[0085] The riser flask 100, the cold mold 400, the lower roll neck flask 500 and the base flask 600 are sequentially connected, and the reliability of the connection can be well ensured by relying on the deadweight of the flask and the cold mold 400 and the cooperation between the groove and the protrusion.
[0086] By cooperating the groove on the top surface of the cold mold 400 with the protrusion on the bottom surface of the riser sand box 100, and the groove on the bottom surface of the cold mold 400 with the protrusion on the top surface of the lower roller neck sand box 500, the centering between the riser sand box 100, the cold mold 400 and the lower roller neck sand box 500 can be ensured, thereby ensuring the concentricity of the axis of the forming roller 900.
[0087] The connection between the gate sand box 200 and the direct pouring sand box 300, as well as the connection between the direct pouring sand box 300 and the base sand box 600, both adopt a U-shaped clamping plate 700. The clamping mouth of the U-shaped clamping plate 700 is provided with an inclined surface. By hammering the U-shaped clamping plate 700 with a hammer or other tools, the clamping mouth can tighten or loosen the connecting part on the gate sand box 200 and the connecting part on the direct pouring sand box 300, and tighten or loosen the connecting part on the direct pouring sand box 300 and the connecting part on the base sand box 600 during the deformation process, thereby realizing quick disassembly and assembly.
[0088] The straight pouring mouth sand box 300 includes a sand box body 310 and a cover plate 320. A U-shaped opening is provided on one side of the sand box body 310, and a cover plate 320 is provided at the U-shaped opening to close the U-shaped opening. The cover plate 320 and the sand box body 310 are fixed by a connecting assembly 330. The connecting assembly 330 includes a T-shaped pull plate 331 and an inclined wedge 332. When connecting the cover plate 320 and the sand box body 310, the T-shaped pull plate 331 is first passed through the sand box body 310 and the cover plate 320, and then the inclined wedge 332 is inserted into the T-shaped pull plate 331. Hitting the inclined wedge 332 with a hammer can make the T-shaped pull plate 331 clamp or loosen the cover plate 320 and the sand box body 310 under the action of the inclined surface deformation of the inclined wedge 332, thereby realizing quick disassembly and assembly.
[0089] Several evenly distributed heat dissipation and exhaust holes are provided on the riser flask 100 , the lower roll neck flask 500 and the base flask 600 , which are beneficial to the solidification of the resin sand and the discharge of hot air when pouring molten iron, thereby ensuring the casting quality of the roll 900 .
[0090] In order to facilitate sand cleaning, the base sand box 600 is hollowed out at the connection with the sprue sand box 300, and a cross-shaped reinforcing rib is provided at the bottom of the base sand box 600 corresponding to the center of the circle of the roller 900. In addition, a counterweight can be provided on the base sand box 600 to adjust the levelness of the base sand box 600.
[0091] See also Figure 6 , an embodiment of the present application provides a method for manufacturing a cast iron roll, comprising:
[0092] Step S1 , molding the riser flask 100 , the gate flask 200 , the sprue flask 300 , the lower roll neck flask 500 and the base flask 600 .
[0093] Step S2, heating the cold mold 400.
[0094] Step S3, assembling the riser flask 100, the gate flask 200, the sprue flask 300, the cold mold 400, the lower roll neck flask 500 and the base flask 600.
[0095] Step S4, detecting the temperature of the cold type 400.
[0096] Step S5, when the temperature of the cold mold 400 is within the preset temperature range, pour molten iron into the pouring port 210 of the pouring flask 200, so that the molten iron first flows from the runner of the sprue flask 300 from top to bottom into the runner of the base flask 600, then flows in the runner of the base flask 600 in a horizontal or inclined direction, and finally spirals up in the base flask 600, the lower roll neck flask 500, the cold mold 400 and the riser flask 100 until the mold cavity is filled.
[0097] In the above steps, the riser flask 100, the gate flask 200, the sprue flask 300, the lower roll neck flask 500 and the base flask 600 are first molded, and then the cold mold 400 is heated, and then the riser flask 100, the gate flask 200, the sprue flask 300, the cold mold 400, the lower roll neck flask 500 and the base flask 600 are combined, and the temperature of the cold mold 400 is detected after the combination. When the temperature of the cold mold 400 is within the preset temperature range, molten iron is poured into the pouring port 210 of the gate flask 200, so that the molten iron first flows from the runner of the sprue flask 300 from top to bottom into the runner of the base flask 600, and then flows into the runner of the base flask 600 in the base flask 600. The molten iron flows in the flow channel of the box 600 in a horizontal or inclined direction, and finally spirally rises in the base sand box 600, the lower roll neck sand box 500, the cold mold 400 and the riser sand box 100 until the cavity is filled. Since the molten iron flows rapidly in the base sand box 600 in a horizontal or inclined direction, and then spirally rises in the base sand box 600, the lower roll neck sand box 500, the cold mold 400 and the riser sand box 100, during this process, impurities such as molten iron slag in the molten iron are brought to the top riser, and impurities such as molten iron slag are located at the top of the forming roll 900. After removing the impurities at the top, there are fewer slag inclusions and fewer pores in the roll 900, thereby improving the overall compactness of the roll 900.
[0098] In steps S4-S5, a thermometer is inserted into the temperature measuring hole 410 of the cold mold 400. When the temperature of the cold mold 400 is detected to be within a preset temperature range of 80-100°C, molten iron is poured into the pouring port 210 of the pouring flask 200.
[0099] In step S5, the time for pouring molten iron is 40-50s; when the molten iron is poured to 3 / 4 of the preset riser height, point pouring is performed until the molten iron is poured to the preset riser height.
[0100] It should be noted that when pouring molten iron, a steady flow is used so that the molten iron is smoothly injected into the pouring port 210 of the pouring flask 200, and finally the molten iron rises relatively steadily in the mold cavity. The overall pouring time of the molten iron can be controlled within 40-50s.
[0101] The preset riser height is lower than the top of the riser sand box 100. When the molten iron is poured to 3 / 4 of the preset riser height, it stays for a while and then is poured in small streams until the height of the molten iron in the cavity reaches the preset riser height.
[0102] After step S5, the method further includes:
[0103] Step S6: Cover the riser with a heat-insulating agent to prevent the riser from shrinking.
[0104] Cover the riser with insulation to improve the riser's shrinkage compensation ability and prevent the riser from shrinking to a certain extent.
[0105] After step S6, the method further includes:
[0106] Step S7: unpack after a preset time.
[0107] In this step, when the diameter of the roller 900 is less than 400 mm, the preset time needs to be greater than 8 hours; when the diameter of the roller 900 is greater than 400 mm, the preset time needs to be greater than 16 hours; at the same time, the temperature of the cold mold 400 should be cooled to 100°C-150°C before unpacking.
[0108] The unpacking sequence is: lift out the gate sand box 200, the sprue sand box 300, the riser sand box 100, and the cold mold 400 from the casting pit in turn, then lift out the roller 900, the lower roll neck sand box 500, and the base sand box 600 as a whole and place them on the sand cleaning site, finally break and separate the sprue section formed in the flow channel of the sprue sand box 300 and the cross gate section formed in the base sand box 600 from the roller 900, clean the appearance of the roller 900, and complete the production of the roller 900 blank.
[0109] Step S8, cleaning the riser flask 100, the gate flask 200, the sprue flask 300, the lower roll neck flask 500 and the base flask 600.
[0110] In this step, the gate sand box 200, the sprue sand box 300, the riser sand box 100, the lower roll neck sand box 500, and the base sand box 600 are placed on the vibration cleaning stand in turn, and the vibrator is turned on. The resin sand begins to fall off under the action of the vibrator until all the resin sand falls off. The various sand boxes are hung in the tooling area for use in the next molding.
[0111] Using a vibrator to clean the resin sand in the sand box is simple to operate, saves manpower, cleans thoroughly and has high cleaning efficiency. You only need to place the sand box on the vibrator and start the vibrator to start cleaning the resin sand. The resin sand will fall off by itself under the vibration of the vibrator and fall onto the screen frame of the vibrator.
[0112] Step S9, recovering the resin sand cleared out of the riser sand box 100, the gate sand box 200, the sprue sand box 300, the lower roll neck sand box 500 and the base sand box 600.
[0113] In this step, the resin sand shaken off the vibrating machine table is sent to the crusher through the conveyor. The crusher will screen the crushed resin sand, separate the useful resin sand for secondary utilization, separate the useless dust and iron blocks for classification and treatment, and the screened useful resin sand will be transported to the storage bin for recycling.
[0114] The resin sand recycling process is adopted to reduce the discharge of industrial waste and reuse the waste industrial waste, which is energy-saving and environmentally friendly. Through the cycle of vibrating sand cleaning, transmission, crushing, screening, storage in different bins, mixing in mixers, sand injection molding and other links, the resin sand is recycled to reduce costs.
[0115] Before step S1, the method further includes:
[0116] The molding sand, furan resin and benzenesulfonic acid curing agent are mixed in proportion by using a sand mixer to form resin sand.
[0117] In this step, the sand mixer can automatically mix the molding sand, environmentally friendly furan resin and environmentally friendly benzenesulfonic acid curing agent according to the required proportion, and then inject them into the parts that need molding through the discharge pipe to complete the injection of resin sand. The useful resin sand screened out in step S9 can also be injected into the parts that need molding through the discharge pipe to achieve secondary utilization of resin sand.
[0118] The advantages of using furan resin to replace the existing earth and sand modeling include at least: the resin sand has good fluidity and does not need to be compacted manually, saving a lot of compaction work; the resin sand can automatically harden within a certain period of time, eliminating the baking mold process and saving energy; the resin sand has good disintegration and is easy to fall off. The sand cleaning work can be completed by simply placing the sand box on a vibrator and vibrating it, eliminating the previous manual cleaning workload; the resin sand recovery rate can reach 90%-95%.
[0119] Please combine Figure 7 , step S1 comprises:
[0120] Sub-step S11, molding the lower roll neck sand box 500: inserting the lower roll neck model 510 into the lower roll neck sand box 500, and making the outer circle stop of the lower roll neck model 510 butt with the inner circle stop of the molding plate 800; injecting resin sand into the lower roll neck sand box 500 by using a sand mixer; and vibrating and compacting the resin sand in the lower roll neck sand box 500 by using a vibrator.
[0121] In the above steps, the molding plate 800 is first placed horizontally, and then the outer circle stop of the lower roller neck model 510 is connected with the inner circle stop of the molding plate 800 to position the lower roller neck model 510, and then the lower roller neck sand box 500 is sleeved on the lower roller neck model 510, and then the prepared resin sand is injected into the lower roller neck sand box 500 through the discharge pipe of the sand mixer, and at the same time, the resin sand in the lower roller neck sand box 500 is vibrated and compacted by a vibrator, and the resin sand is placed and vibrated until the resin sand is flush with the plane of the lower roller neck sand box 500 away from the molding plate 800.
[0122] Please combine Figure 8 , after sub-step S11, further comprising:
[0123] Sub-step S12, molding the base sand box 600: setting the base sand box 600 on the lower roll neck sand box 500; pre-embedding the runner white mold in the base sand box 600, so that the runner white mold is tangent to the outer circle of the lower roll neck model 510; injecting resin sand into the base sand box 600 by using a sand mixer; and vibrating and compacting the resin sand in the base sand box 600 by using a vibrator.
[0124] In the above steps, after the resin sand in the lower roll neck sand box 500 is hardened, the base sand box 600 is turned upside down on the lower roll neck sand box 500, and the bayonet on the base sand box 600 and the lower roll neck sand box 500 are aligned for positioning, and a temporary molding plugging steel plate 610 is placed at the connection position between the base sand box 600 and the sprue sand box 300, the bottom of the temporary molding plugging steel plate 610 is padded with a supporting square box 620 for leveling, and a cross runner white mold is pre-embedded in the base sand box 600, and finally a sand mixer is used to inject resin sand into the cavity of the base sand box 600, and vibrated and compacted by a vibrator. After the resin sand in the lower roll neck sand box 500 and the base sand box 600 is solidified, they are successively lifted out and turned 180° for placement, and the lower roll neck model 510 is taken out and put aside for use when the boxes are closed.
[0125] Among them, a white foam model, namely a cross runner white mold, is embedded in the base sand box 600, and the cross runner white mold is fixed in the base sand box 600, and the cross runner white mold is made tangent to the outer circle of the lower roll neck model 510. When the molten iron melts the cross runner white mold, a flow channel is rushed out in the base sand box 600. The molten iron enters the mold cavity along the flow channel in the base sand box 600, and gradually fills the top of the riser in a spiral upward flow manner. During this period, impurities such as molten iron slag can be brought to the top of the riser to ensure the tightness of the roller 900 body and avoid defects such as pores and slag inclusions.
[0126] Please combine Fig. 9 , step S1 further includes:
[0127] Sub-step S13, molding the riser sand box 100: inserting the upper roller neck model 110 into the riser sand box 100, and making the outer circle stop of the upper roller neck model 110 butt with the inner circle stop of the molding plate 800; injecting resin sand into the riser sand box 100 by using a sand mixer; and vibrating and compacting the resin sand in the riser sand box 100 by using a vibrator.
[0128] In this step, the outer circle stop of the upper roll neck model 110 is placed into the inner circle stop of the molding plate 800 to position the upper roll neck model 110, and then the riser sand box 100 is sleeved on the upper roll neck model 110 and placed on the molding plate 800, and the convex surface of the riser sand box 100 is aligned with the concave surface of the molding plate 800 for positioning. Then, the prepared resin sand is injected into the riser sand box 100 from the discharge pipe of the sand mixer, and vibrated and compacted by a vibrator until the resin sand in the riser sand box 100 is flush with the top plane of the riser sand box 100. After the resin sand in the riser sand box 100 is hardened, the upper roll neck model 110 is taken out and put into use when the box is closed.
[0129] It should be noted that the upper roll neck model 110 is consistent with the shape of the upper roll neck of the formed roll 900 blank, and a breaking length of 400-600 mm is reserved at the top of the roll 900 blank. After the casting of the roll 900 is completed, it is first processed and cut off and then broken and removed with a heavy hammer to eliminate the influence of pores and impurity defects; the upper roll neck model 110 and the lower roll neck model 510 are both made of castings. In order to reduce the weight of the upper roll neck model 110 and the lower roll neck model 510, the interiors of the upper roll neck model 110 and the lower roll neck model 510 are both hollow structures.
[0130] The concave inner ring on the molding plate 800 is also provided with another concave surface, namely the inner ring stop of the molding plate 800 , through which the inner ring stop of the molding plate 800 cooperates with the outer circle stop of the upper roller neck model 110 to position the upper roller neck model 110 .
[0131] Step S1 also includes:
[0132] Sub-step S14, molding the sprue sand box 300: placing the sprue sand box 300 horizontally on the molding site; setting a sprue white mold in the sprue sand box 300; injecting resin sand into the sprue sand box 300 by a sand mixer; and vibrating and compacting the resin sand in the sprue sand box 300 by a vibrator.
[0133] In this step, first place the sprue sand box 300 with its side opening facing upward on the molding site, then place the sprue white mold in the sprue sand box 300 and fix it, then inject resin sand into the sprue sand box 300, and then scrape the mortar surface at the side opening of the sprue sand box 300 flat, after the resin sand in the sprue sand box 300 is solidified, cover the side opening of the sprue sand box 300 with a cover plate 320, and fix the cover plate 320 by a T-shaped pull plate 331 and an inclined wedge 332.
[0134] Among them, the sprue white mold is butted against the runner white mold, and an arc transition is adopted at the butt joint between the sprue white mold and the runner white mold. On the one hand, it can prevent the resin sand in the base sand box 600 from collapsing when the molten iron is poured, and on the other hand, it can also increase the flow rate of the molten iron to ensure the pouring quality. The sprue white mold and the runner white mold will melt directly when the molten iron is poured, which is more convenient than the existing method of pre-embedded steel pipes and then pulled out, thereby improving the casting quality of the rolling roller 900.
[0135] Step S1 also includes:
[0136] Sub-step S15, molding the gate sand box 200: placing the gate sand box 200 on a molding site; setting a gate model in the gate sand box 200; injecting resin sand into the gate sand box 200 using a sand mixer; and vibrating and compacting the resin sand in the gate sand box 200 using a vibrator.
[0137] It should be noted that the gate sand box 200 is also molded by resin sand casting. After molding, the gate model in the gate sand box 200 is taken out, and the inner wall of the preset pouring port 210 in the gate sand box 200 is painted to prevent it from being burned by molten iron. The preset pouring port 210 in the gate sand box 200 should be aligned with the runner position in the straight gate sand box 300 to avoid misalignment.
[0138] Step S2 includes:
[0139] Sub-step S21, placing the cold mold 400 in a box-type resistance furnace and heating it to 140-160° C. and maintaining a constant temperature.
[0140] Sub-step S22, applying paint inside the cold mold 400 and maintaining a constant temperature, wherein the paint includes coke powder, graphite powder and syrup, and the ratio of coke powder, graphite powder and syrup is 5:3:2.
[0141] Before the cold mold 400 is heated, the inside of the cold mold 400 needs to be polished clean with an electric brush to remove the old paint. About an hour before the casting of the roller 900, the paint is applied to the inside of the cold mold 400 and the temperature is kept constant.
[0142] Step S3 includes: stacking the base sand box 600, the cold mold 400, the riser sand box 100, the sprue sand box 300, and the gate sand box 200 in the casting pit in sequence; fixing the sprue sand box 300 and the base sand box 600 with bolts; fixing the gate sand box 200 and the sprue sand box 300 with bolts.
[0143] Before assembling the boxes, check that the gate sand box 200, the sprue sand box 300, the base sand box 600, the cold mold 400 and the riser sand box 100 are kept clean without any residual floating sand. For thorough cleaning, use the leather hose connected to the negative pressure box to suck away the fine sand and dust on the surface of the sand box and the cold mold 400.
[0144] The pit casting method is adopted, and the casting tooling is placed in the casting pit. A safety guardrail is set in the casting pit. Operators only need to stand on the ground to perform the casting operation, which is safe and convenient. Stairs are set in the casting pit so that personnel can walk from the casting pit to the ground.
[0145] The base sand box 600, the cold mold 400, the riser sand box 100, the sprue sand box 300, and the gate sand box 200 are stacked in the pouring pit in sequence, and the contact surfaces between the sand boxes are tightly connected to avoid sparks during pouring and the formation of defects such as flash and burrs; finally, the base sand box 600 is fixed to the sprue sand box 300 with bolts, and the sprue sand box 300 is fixed to the gate sand box 200 with bolts to complete the box assembly.
[0146] Before step S5, the method also includes: smelting molten iron in a medium frequency furnace; pouring the molten iron into a ladle; and hoisting the ladle to the top of the pouring pit by a crane.
[0147] Before pouring molten iron, it is necessary to melt molten iron in a medium frequency furnace, put in pig iron and alloy of the required proportion according to the components required by the rolling roller 900, heat it to about 1450℃, remove the slag, and put 2% spheroidizing agent (rare earth silicon iron magnesium alloy) and 0.6% inoculant (75Si-Fe) in the ladle in advance. After the molten iron is taken out of the furnace, it is poured into the ladle for spheroidization and inoculation. After the molten iron is fully stirred and removed in the ladle, it is necessary to first pour a molten iron test block to check the spheroidization. After the molten iron test block is inspected and qualified, 0.1% inoculant (75Si-Fe) is added to the ladle for floating silicon inoculation. Before pouring, the molten iron pouring temperature is controlled at 1250-1300℃. In addition, before pouring molten iron, a thermometer is inserted into the temperature measuring hole 410 of the cold mold 400 for temperature measurement. If the temperature is 80-100℃, it meets the pouring temperature.
[0148] To summarize, the embodiments of the present application provide a method for manufacturing a cast iron roll and a casting tool. In the method for manufacturing a cast iron roll, the molten iron flows rapidly in the flow channel in the base sand box 600, and then spirally rises in the base sand box 600, the lower roll neck sand box 500, the cold mold 400 and the riser sand box 100. During this process, impurities such as molten iron slag in the molten iron are brought to the top riser, and impurities such as molten iron slag are located at the top of the forming roll 900. The roll 900 except the top has less slag inclusions and fewer pores, thereby improving the overall compactness of the roll 900.
[0149] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for manufacturing a cast iron roll, characterized in that: Applied to a casting tool, the casting tool comprises a riser flask, a sprue flask, a direct sprue flask, a cold mold, a lower roll neck flask and a base flask, the lower roll neck flask and the direct sprue flask are both arranged on the top of the base flask, and the lower roll neck flask is located on one side of the direct sprue flask in the horizontal direction, the cold mold is arranged on the top of the lower roll neck flask, the riser flask is arranged on the top of the cold mold, the sprue flask is arranged on the top of the direct sprue flask, a pouring port is arranged in the sprue flask, a connected flow channel is arranged in the direct sprue flask and the base flask, and the base flask, the lower roll neck flask and the riser flask are connected to form a cavity; The manufacturing method comprises: Molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask; heating the cold type; Combining the riser flask, the gate flask, the sprue flask, the cold mold, the lower roll neck flask and the base flask; Detecting the temperature of the cold type; When the temperature of the cold mold is within a preset temperature range, molten iron is poured into the pouring port of the pouring flask, so that the molten iron first flows from the runner of the sprue flask into the runner of the base flask from top to bottom, then flows in the runner of the base flask, and finally spirally rises in the base flask, the lower roll neck flask, the cold mold and the riser flask until the mold cavity is filled.
2. The method for manufacturing a cast iron roll according to claim 1, characterized in that: In the step of pouring molten iron into the pouring port of the pouring flask, the pouring time of the molten iron is 40-50 seconds; When the molten iron is poured to 3 / 4 of the preset riser height, point pouring is performed until the molten iron is poured to the preset riser height.
3. The method for manufacturing a cast iron roll according to claim 2, characterized in that: After the step of pouring molten iron into the pouring port of the pouring flask, the method further comprises: Cover the riser with insulation to prevent the riser from shrinking.
4. The method for manufacturing a cast iron roll according to claim 3, characterized in that: After the step of covering the riser with the insulation agent, the step further includes: Unboxing is performed after a preset time; Cleaning the riser sand box, the gate sand box, the sprue sand box, the lower roll neck sand box and the base sand box; The resin sand cleared out of the riser sand box, the gate sand box, the sprue sand box, the lower roll neck sand box and the base sand box is recovered.
5. The method for manufacturing a cast iron roll according to claim 1, characterized in that: Before the step of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask, the method further includes: The molding sand, furan resin and benzenesulfonic acid curing agent are mixed in proportion by using a sand mixer to form resin sand.
6. The method for manufacturing a cast iron roll according to claim 1, characterized in that: The step of heating the cold profile comprises: Place the cold mold in a box-type resistance furnace and heat it to 140-160°C and keep the temperature constant; A coating is applied inside the cold mold and maintained at a constant temperature, wherein the coating comprises coke powder, graphite powder and syrup, and the ratio of the coke powder, the graphite powder and the syrup is 5:3:
2.
7. The method for manufacturing a cast iron roll according to claim 1, characterized in that: The steps of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask include: The lower roll neck flask is molded: Insert the lower roll neck model into the lower roll neck sand box, and make the outer circle stop of the lower roll neck model butt with the inner circle stop of the molding plate; Injecting resin sand into the lower roll neck sand box by using a sand mixer; The resin sand in the lower roll neck sand box is vibrated and compacted by a vibrator.
8. The method for manufacturing a cast iron roll according to claim 7, characterized in that: After the step of shaping the lower roll neck flask, it also includes: The base sand box is molded: The base flask is arranged on the lower roll neck flask; Pre-embedding a runner white mold in the base sand box so that the runner white mold is tangent to the outer circle of the lower roll neck model; Injecting resin sand into the base sand box using a sand mixer; The resin sand in the base sand box is vibrated and compacted by using a vibrator.
9. The method for manufacturing a cast iron roll according to claim 1, characterized in that: The steps of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask include: The riser sand box is molded: Inserting the upper roll neck model into the riser sand box, and making the outer circle stop of the upper roll neck model butt with the inner circle stop of the molding plate; Injecting resin sand into the riser sand box using a sand mixer; The resin sand in the riser sand box is vibrated and compacted by using a vibrator.
10. The method for manufacturing a cast iron roll according to claim 1, characterized in that: The steps of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask include: The sprue sand box is molded: Placing the sprue sand box horizontally on the molding site; Arranging a sprue white mold in the sprue sand box; Injecting resin sand into the sprue sand box using a sand mixer; The resin sand in the sprue sand box is vibrated and compacted by using a vibrator.
11. The method for manufacturing a cast iron roll according to claim 1, characterized in that: The steps of molding the riser flask, the gate flask, the sprue flask, the lower roll neck flask and the base flask include: The gate sand box is molded: Placing the pouring sand box on a molding site; Arranging a gate model in the gate sand box; Injecting resin sand into the pouring sand box using a sand mixer; The resin sand in the pouring sand box is vibrated and compacted by using a vibrator.
12. The method for manufacturing a cast iron roll according to claim 1, characterized in that: The step of combining the riser flask, the gate flask, the sprue flask, the cold mold, the lower roll neck flask and the base flask comprises: The base sand box, the cold mold, the riser sand box, the sprue sand box, and the gate sand box are stacked and assembled in sequence in the casting pit; Fixing the sprue sand box and the base sand box with bolts; The gate sand box and the sprue sand box are fixed with bolts.
13. The method for manufacturing a cast iron roll according to claim 1, characterized in that: Before the step of pouring molten iron into the pouring port of the pouring flask, the method further comprises: Melting molten iron in a medium frequency furnace; Pour molten iron into a ladle; Use a crane to lift the molten iron ladle to the top of the casting pit.
14. A casting tool, characterized in that: It includes a riser sand box, a pouring gate sand box, a straight gate sand box, a cold mold, a lower roller neck sand box and a base sand box. The lower roller neck sand box and the straight gate sand box are both arranged on the top of the base sand box, and the lower roller neck sand box is located on one side of the straight gate sand box in the horizontal direction. The cold mold is arranged on the top of the lower roller neck sand box, the riser sand box is arranged on the top of the cold mold, the pouring gate sand box is arranged on the top of the straight gate sand box, a pouring gate is arranged in the pouring gate sand box, and the straight gate sand box and the base sand box are arranged with connected runners, and the base sand box, the lower roller neck sand box and the riser sand box are connected to form a mold cavity.
15. The casting tool according to claim 14, characterized in that: A temperature measuring hole is provided on the side of the cold mold, grooves are provided on the top and bottom surfaces of the cold mold, protrusions are provided on the top surface of the lower roller neck flask and the bottom surface of the riser flask, the groove on the top surface of the cold mold cooperates with the protrusion on the bottom surface of the riser flask, and the groove on the bottom surface of the cold mold cooperates with the protrusion on the top surface of the lower roller neck flask, so as to ensure the centration among the riser flask, the cold mold and the lower roller neck flask.