Low-pressure casting method and mold for water pump shell
By using built-in shunt pack and rapid boosting crystallization process in low-pressure casting of aluminum alloy water pump housing, the problems of low yield and filling and solidification defects in the existing technology are solved, and high quality and high efficiency are achieved. Casting production.
Patent Information
- Application Number
- CN202411571261.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-03
Smart Images

Figure CN119057039A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of automobile parts casting, and in particular to a low-pressure casting method and a mold for a water pump housing. Background Art
[0002] With the deepening of the trend of lightweight automobiles, more and more automobile metal parts are changed from steel parts to aluminum alloy parts. Among them, a large number of small parts are constantly developing related casting molds to improve production efficiency and reduce production costs. The aluminum alloy low-pressure casting process has many advantages and is increasingly widely used. At present, there are relatively mature processes for low-pressure casting of aluminum alloy automobile wheels, low-pressure casting of aluminum alloy cylinder blocks and cylinder heads on automobile engines, low-pressure casting of intake manifolds, and low-pressure casting of flywheel housings. Low-pressure casting of small castings has also been widely used in production practice.
[0003] Although the casting mold in the prior art can cast a well-formed workpiece, there are problems such as low process yield, low production efficiency and high production cost. In addition, there are often obvious defects in filling and solidification shrinkage. Summary of the invention
[0004] The present invention aims to solve the above technical problems by connecting a built-in diverter bag at the injection port of the cavity to ensure that the molten metal fills the cavity when the diverter bag is depressurized, so that the obtained workpiece has better quality and a higher process yield.
[0005] To achieve the above-mentioned purpose, the present invention provides a low-pressure casting method for a water pump housing. The low-pressure casting method is applied to a low-pressure casting mold. The low-pressure casting mold includes an upper mold insert, a lower mold insert, a built-in diverter bag and a gate sleeve. The low-pressure casting method includes: cooperating the upper mold insert and the lower mold insert with each other to form a cavity; injecting molten metal from the gate sleeve into the built-in diverter bag and sending it to the interior of the built-in diverter bag; the molten metal enters and fills the cavity along the inner gate.
[0006] The low-pressure casting method for water pump housing provided in this embodiment can reduce the turbulence and gas inclusions generated by the molten metal during the filling process, thereby reducing the porosity and inclusion defects of the casting, and improving the mechanical properties and appearance quality of the product, wherein the built-in diverter bag can play an effective shrinkage compensation effect. The casting cavity is formed by the precise matching of the upper and lower mold inserts, and the cavity accurately defines the shape and size of the final product. The molten metal is first injected into the gate sleeve, which is used to temporarily store and guide the molten metal. The molten metal flows from the gate sleeve to the built-in diverter bag, which is a channel connecting the gate sleeve and the cavity, and plays a role in guiding the molten metal. The molten metal is injected along the inner gate and evenly fills the cavity, and finally forms a water pump housing with no internal defects and good quality.
[0007] In any of the above technical solutions, when the cavity is filled, the built-in diversion package is pressurized to achieve a state where the molten metal replenishes the cavity.
[0008] When the cavity is filled with molten metal, the built-in diverter bag increases the pressure to achieve a state where the molten metal replenishes the cavity. Under this condition, more molten metal can enter and fill the cavity, reducing defects caused by filling, solidification and shrinkage. The molten metal replenishing the cavity can ensure a smooth surface when the molten metal fills the cavity, reduce defects caused by bubbles and gas, and improve the surface quality and qualified rate of the casting. After the product solidifies and forms in the cavity, the built-in diverter bag releases the pressure to achieve an empty state, improving the casting process yield rate.
[0009] In any of the above technical solutions, the initial pouring temperature of the water pump housing is controlled at 680°C-750°C; and / or the casting temperature of the water pump housing is controlled at 350°C-450°C.
[0010] In the casting process, the initial pouring temperature refers to the temperature before the molten metal is poured into the mold. It is controlled at 680℃ to 750℃ to ensure that the molten metal has enough thermal energy during the flow process so that it can effectively fill the fine structure and complex shape of the mold. Within this temperature range, the viscosity of the molten metal decreases, making it more fluid, which helps to ensure that the molten metal evenly fills the cavity and reduces the generation of air and bubbles.
[0011] Through the low-pressure casting mold, under the influence of the heat capacity of the built-in diverter package, the casting temperature of the water pump housing is controlled between 350℃-450℃. Within this temperature range, it can be ensured that the molten metal reaches appropriate fluidity and solidification speed in the process of filling the cavity, thereby realizing the precise molding of the casting, basically eliminating defects such as cold shut and insufficient pouring of the casting, and can effectively compensate for shrinkage, thereby improving the quality and reliability of the product. At the same time, this temperature range also helps to achieve metal solidification within an appropriate time, ensuring the structural stability and consistency of the casting.
[0012] In any of the above technical solutions, the low-pressure casting method adopts a rapid pressurization crystallization process, which includes: a liquid rising stage, a mold filling stage, a pressurization stage, a pressure holding stage and a pressure relief stage.
[0013] In the liquid raising stage, the molten metal is gradually raised to the casting mold through the low-pressure system to prepare for the subsequent filling. This stage ensures that the molten metal enters the cavity stably and evenly. In the filling stage, the molten metal fills the cavity at a high speed. This stage requires precise control of the flow rate and pressure to ensure that the cavity is fully filled and reduce the possibility of gas inclusions and other defects. The pressurization stage promotes the rapid crystallization of the molten metal by rapidly increasing the pressure, ensuring the formation of a fine and uniform grain structure inside the casting. This process has an important influence on the strength and toughness of the casting. The pressure holding stage maintains a certain pressure to ensure the complete solidification and crystallization of the molten metal, thereby improving the density of the casting and reducing the risk of internal stress and deformation. The pressure relief stage safely releases the pressure inside the cavity through the decompression operation, preparing for the removal of the casting and ensuring the integrity and surface quality of the casting.
[0014] The rapid pressure crystallization process can significantly improve the microstructure of the casting, reduce pores, inclusions and other defects, thereby improving the overall quality and performance of the casting. By optimizing the crystallization process, the process can improve the mechanical properties of the casting, enhance its strength, toughness and corrosion resistance, and meet higher use requirements.
[0015] In any of the above technical solutions, the liquid lifting pressure in the liquid lifting stage is 0.018MPa-0.022MPa, and the liquid lifting time is 2s-4s; and / or the filling pressure in the filling stage is 0.026MPa-0.03MPa, and the filling time is 7s-9s; and / or the boosting pressure in the pressurization stage is 0.033MPa-0.037MPa, and the pressurization time is 1s-3s; and / or the holding pressure in the holding stage is 0.033MPa-0.037MPa, and the holding time is 65s-75s; and / or the pressure relief time in the pressure relief stage is 4s-6s.
[0016] In the liquid raising stage, appropriate liquid raising pressure and time are used to ensure that the metal liquid rises to the cavity stably and evenly, reducing the generation of bubbles. In the filling stage, the filling pressure and time are controlled to ensure that the metal liquid fills the cavity quickly and evenly, thereby improving the filling efficiency of the cavity and the surface quality of the casting. In the pressurization stage, the crystallization process of the metal liquid is accelerated by increasing the pressure, which promotes the formation of a more uniform and delicate grain structure. In the pressure holding stage, the metal liquid is completely solidified by maintaining appropriate pressure and time, improving the density and overall quality of the casting. In the pressure relief stage, the pressure in the cavity is safely released through a reasonable pressure relief time, preparing for the removal of the casting and reducing the risk of deformation.
[0017] The present invention also provides a low-pressure casting mold for a water pump housing. The low-pressure casting mold adopts the low-pressure casting method as described above. The low-pressure casting mold includes: an insert, the insert includes an upper mold insert and a lower mold insert, the upper mold insert and the lower mold insert cooperate with each other to form a cavity; a built-in diverter bag, and an internal gate is arranged around the built-in diverter bag; a gate sleeve, and the gate sleeve is connected to the internal space of the built-in diverter bag to deliver the molten metal from the gate sleeve to the built-in diverter bag and fill the cavity.
[0018] The low-pressure casting mold for manufacturing a water pump housing provided by the present invention is provided with a built-in diverter bag inside the low-pressure casting mold, and the built-in diverter bag is connected with the cavity through an inner gate, so that the molten metal in the built-in diverter bag is evenly delivered to the cavity, wherein the built-in diverter bag can better fill the defects in the cavity with the molten metal by pressurizing the molten metal, thereby improving the quality of the product; the molten metal inside the built-in diverter bag is emptied by pressure relief, thereby improving the process yield. The specific shape of the water pump housing is formed by cooperating the upper mold insert and the lower mold insert with each other to form a plurality of cavities; the inner gate is provided around the built-in diverter bag, so that the molten metal can be guided into the cavity, ensuring the smooth progress of the filling process; the gate sleeve is provided to deliver the molten metal from the gate sleeve to the built-in diverter bag, and finally fill the cavity, which is conducive to ensuring that the molten metal is evenly distributed in the cavity and avoiding the occurrence of voids or other defects.
[0019] The design of the built-in diverter bag enables the molten metal to be filled into the cavity more smoothly, thereby speeding up the casting process and improving production efficiency; by ensuring uniform filling and flow of the molten metal, the mold helps to reduce defects in the casting and improve the quality of the final product; due to the improvement in production efficiency and optimization of casting quality, the use of the mold provided by the present invention can reduce production costs and increase the economic benefits of production.
[0020] In any of the above technical solutions, an annular runner is provided inside the built-in diversion package, and the annular runner surrounds and defines a cavity structure.
[0021] The design of the annular runner means that the molten metal can flow in a continuous annular path, thereby surrounding and defining a central cavity structure, and the cavity structure is conducive to the internal distribution of the built-in diverter bag. Among them, the design of the annular runner can allow the molten metal to enter the mold cavity evenly, thereby achieving more uniform filling and reducing pores and inclusions in the casting; the annular runner can reduce the eddy currents generated when the molten metal enters the cavity, reduce the possibility of slag mixing, and help maintain the purity of the casting; the annular runner can increase the filling speed of the molten metal, allowing it to fill the cavity faster, thereby shortening the production cycle. The formation of the cavity structure provides a basis for the built-in diverter bag to relieve pressure and empty, thereby ensuring that the molten metal of the gate sleeve enters the cavity through the built-in diverter bag and effectively fills the surrounding area of the cavity, thereby improving the overall quality of the casting and avoiding defects caused by uneven filling of the molten metal.
[0022] In any of the above technical solutions, the built-in diverter bag is provided with a thermal insulation coating; and / or a plurality of heating tubes are provided inside the insert; and / or each cavity is connected to two inner gates.
[0023] The thermal insulation coating in the present invention is a special coating applied to the surface of the built-in shunt bag, and its main function is to provide thermal insulation effect. The thermal insulation coating can effectively reduce the heat loss, thereby improving the temperature stability of the built-in shunt bag. During the casting process, maintaining a stable temperature is crucial to ensure the fluidity and filling of the molten metal; since the thermal insulation coating reduces the conduction and loss of heat, the energy required in the casting process is relatively less, which is conducive to reducing the energy cost of the casting process and improving production efficiency; the thermal insulation coating can keep the surface of the built-in shunt bag at a relatively high temperature, which helps to reduce the solidification and cooling of the molten metal, thereby improving the fluidity and filling of the molten metal; by keeping the surface temperature of the built-in shunt bag stable, the thermal insulation coating can reduce casting defects caused by temperature changes, such as cold cracks, pores and shrinkage defects, which is conducive to improving the quality and reliability of castings; the thermal insulation coating can reduce the thermal stress and thermal shock on the surface of the built-in shunt bag, thereby extending the service life of the built-in shunt bag and reducing the maintenance and replacement costs of the equipment.
[0024] The insert is an important part of the low-pressure casting mold. It is used to contain the molten metal and form the shape of the casting. By designing multiple heating tubes inside the insert to heat the insert and the molten metal, the temperature inside the insert reaches the required casting temperature. The heat energy provided by the heating tube can effectively control the temperature of the molten metal, reduce the temperature gradient and thermal stress, thereby reducing the internal defects of the casting and improving the casting quality; compared with the traditional overall heating method, the internal heating tube can more effectively transfer heat energy to the molten metal and the mold, reduce energy waste, and reduce energy costs; reasonable temperature control can reduce the thermal stress and wear of the mold, extend the service life of the mold, and reduce replacement costs and production interruptions; stable casting temperature can ensure the consistency of the quality and performance of each casting, and enhance the consistency and reliability of the product.
[0025] By connecting two ingates to each cavity, the molten metal can enter the cavity from two different directions, which helps the molten metal flow in the cavity, making the filling more uniform and effectively reducing casting defects such as pores and shrinkage caused by uneven filling of the molten metal. The setting of two ingates speeds up the filling of the molten metal, shortens the entire casting cycle, and is conducive to improving production efficiency, especially in a large-scale production environment, which can significantly increase production; the use of two ingates can also reduce the internal stress caused by uneven temperature caused by the flow of molten metal, and reduce the risk of warping and deformation of castings; the introduction of molten metal from two different directions helps the structural uniformity of the metal during the solidification process, and improves the mechanical properties and durability of the casting.
[0026] In any of the above technical solutions, the thickness of the thermal insulation coating ranges from 3mm to 3.5mm.
[0027] By specifying the thickness range of the insulation coating, it is possible to ensure that there is sufficient insulation layer on the surface of the built-in shunt package to reduce heat loss. Selecting the appropriate thickness within the specified range can optimize the insulation effect and ensure temperature stability during the casting process. The regulation of the thickness range of the insulation coating can avoid excessive use of materials, thereby saving costs. By ensuring that the coating thickness is within a reasonable range, the material can be maximized while meeting the insulation requirements. The selection of the thickness range of the insulation coating may take into account the load-bearing capacity of the surface of the built-in shunt package. The appropriate coating thickness can reduce the load on the surface of the built-in shunt package, extend the life of the equipment and reduce maintenance costs. By applying the insulation coating within the appropriate thickness range, the efficiency and stability of the casting process can be improved. The stable temperature helps to maintain the fluidity and quality of the molten metal, thereby improving production efficiency and reducing production interruptions. The appropriate thickness of the insulation coating can ensure that the molten metal maintains a stable temperature when filling the mold, thereby reducing the occurrence of casting defects.
[0028] In any of the above technical solutions, the low-pressure casting mold also includes a top plate and a bottom plate, the top plate is arranged on a side close to the upper mold insert, and the bottom plate is arranged on a side close to the lower mold insert.
[0029] The top plate and bottom plate are components of the low-pressure casting mold. The top plate is located on one side of the upper mold insert, and the bottom plate is located on one side of the lower mold insert. The position and adjustment between the top plate and the bottom plate affect the gap size between the upper mold insert and the lower mold insert, thereby controlling the flow and filling of the molten metal during the casting process. Through the adjustment of the top plate, the mold gap during the casting process can be accurately controlled, thereby achieving accurate casting of the casting shape and size, which is beneficial to improving the quality and consistency of the casting; accurate adjustment can reduce the waste of molten metal and the occurrence of casting defects during the casting process. By ensuring the appropriate gap between the molds, the leakage and insufficient filling of the molten metal can be reduced, and the scrap rate can be reduced; optimizing the mold adjustment design can reduce production costs and reduce the scrap rate and losses caused by production interruptions.
[0030] After adopting the technical solution of the present invention, the following technical effects can be achieved: (1) The built-in diverter bag can effectively compensate for the shrinkage of the casting, and has a significant effect on eliminating defects such as cold shut and insufficient pouring for thin-walled castings; (2) Thickening the insulation coating layer of the built-in diverter bag and venting the built-in diverter bag after pressure relief can achieve a higher process yield; (3) The volume of aluminum liquid in the built-in diversion package is relatively large, which will have a greater impact on the mold temperature and is more suitable for casting small castings; however, for medium and large castings, it may cause the mold temperature to be too high, thereby affecting production efficiency and causing casting defects when the pressure is released and the runner is emptied. Therefore, this process is suitable for small castings, but not for medium and large castings. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which: Figure 1 A schematic cross-sectional view of a low-pressure casting mold provided by an embodiment of the present invention from a main viewing angle; Figure 2 A schematic cross-sectional view from a top view of a low-pressure casting mold provided by an embodiment of the present invention; Figure 3 A schematic cross-sectional view of a lower mold insert from a main viewing angle provided by an embodiment of the present invention; Figure 4 A top view of a lower mold insert provided by an embodiment of the present invention; Figure 5 A schematic cross-sectional view of the upper mold insert from a main viewing angle provided by an embodiment of the present invention; Figure 6A top view of a lower mold insert provided by an embodiment of the present invention; Figure 7 A schematic cross-sectional view of a sprue bushing from a main viewing angle provided by an embodiment of the present invention; Figure 8 A pressure curve diagram of a rapid pressurization crystallization process provided by an embodiment of the present invention; Fig. 9 A low-pressure casting diagram of a water pump housing provided by an embodiment of the present invention; Fig.10 A schematic diagram of an ideal state of emptying the low-pressure runner of a water pump housing provided by an embodiment of the present invention; Fig.11 A solidification simulation analysis diagram of a water pump housing provided by an embodiment of the present invention; Fig.12 A low-pressure casting product sample of a water pump casing provided in an embodiment of the present invention.
[0032] Description of reference numerals: 100-insert; 110-upper mold insert; 120-lower mold insert; 130-cavity; 140-heating tube; 200-built-in diverter package; 210-inner gate; 220-annular runner; 300-gate bushing; 400-top plate; 500-bottom plate. DETAILED DESCRIPTION
[0033] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] On a low-pressure casting machine with a single-lift liquid pipe, if the mold needs multiple gates for pouring, a diverter bag needs to be added between the mold and the furnace cover, which is generally called a pouring basin at the production site. However, the pouring basin has many defects in actual production applications, such as the large volume of the pouring basin resulting in a large amount of aluminum liquid returning to the furnace, and the lowering of the temperature of the aluminum liquid in the pouring basin will cause defects such as cold shut, insufficient pouring, and gate freezing of the casting. Therefore, for medium and large castings, multi-gate casting is now mostly developing in the direction of multi-lift liquid pipe furnace covers.
[0035] For small castings, multiple gates are obviously not suitable for pouring. Therefore, in the process of process design and verification, this embodiment proposes the concept of built-in diverter bag, which is actually the result of enlarging the horizontal runner in the mold cavity and evolving into a similar pouring basin. Through production verification, the final casting obtained a water pump housing with a high process yield.
[0036] An embodiment of the present invention provides a low-pressure casting method for a water pump housing. The low-pressure casting method is applied to a low-pressure casting mold. The low-pressure casting mold includes an upper mold insert, a lower mold insert, a built-in diverter package and a gate sleeve. The low-pressure casting method includes: cooperating the upper mold insert and the lower mold insert with each other to form a cavity; injecting molten metal from the gate sleeve into the built-in diverter package and sending it to the interior of the built-in diverter package; the molten metal enters and fills the cavity along the inner gate.
[0037] The low-pressure casting method for water pump housing provided by the present invention can reduce the turbulence and gas inclusions generated by the molten metal during the filling process, thereby reducing the pores and inclusion defects of the casting, and improving the mechanical properties and appearance quality of the product, wherein the built-in diverter bag can play an effective shrinkage compensation effect. The casting cavity is formed by the precise matching of the upper and lower mold inserts, and the cavity accurately defines the shape and size of the final product. The molten metal is first injected into the gate sleeve, which is used to temporarily store and guide the molten metal. The molten metal flows from the gate sleeve to the built-in diverter bag, which is a channel connecting the gate sleeve and the cavity, and plays a role in guiding the molten metal. The molten metal is injected along the inner gate and evenly fills the cavity, and finally forms a water pump housing with no internal defects and good quality.
[0038] The low-pressure casting process is mainly used for casting aluminum alloy product blanks. The molten metal liquid is filled into the mold from bottom to top in the opposite direction of gravity under the action of gas pressure in a sealed insulation furnace. The filling is smooth, which can avoid tumbling, impact and splashing, and reduce oxidation slag inclusions; the fluidity is increased, which is convenient for pouring complex thin-walled castings and makes the casting contour clear; the casting crystallizes and solidifies under pressure, and can get sufficient shrinkage compensation, so the casting has a dense structure and high mechanical properties, and high-quality castings can be obtained, and the qualified rate can generally reach more than 90%. The pouring system of low-pressure casting is relatively simple, which can reduce or eliminate risers. The unsolidified molten metal can flow back to the crucible to reduce metal loss, so the process yield is high, up to 75%-95%; high production efficiency, small subsequent processing allowance, and less machining time; wide range of applications, can produce various castings of different materials, sizes, structures, and wall thicknesses; easy to realize mechanical automated production, productivity is 2-3 times higher than that of metal molds, workers have low labor intensity and better working conditions; low-pressure casting has higher equipment investment and mold costs than metal mold casting, higher requirements on production site process conditions, and strict control requirements on various process parameters.
[0039] In some embodiments of the present application, when the cavity is filled, the built-in diversion package is pressurized to achieve a state in which the molten metal replenishes the cavity.
[0040] When the cavity is filled with molten metal, the built-in diverter bag increases the pressure to achieve a state where the molten metal replenishes the cavity. Under this condition, more molten metal can enter and fill the cavity, reducing defects caused by filling, solidification and shrinkage. The molten metal replenishing the cavity can ensure a smooth surface when the molten metal fills the cavity, reduce defects caused by bubbles and gas, and improve the surface quality and qualified rate of the casting. After the product solidifies and forms in the cavity, the built-in diverter bag releases the pressure to achieve an empty state, improving the casting process yield rate.
[0041] In some embodiments of the present application, the initial pouring temperature of the water pump housing is controlled at 680°C-750°C; and / or the casting temperature of the water pump housing is controlled at 350°C-450°C.
[0042] In the casting process, the initial pouring temperature refers to the temperature before the molten metal is poured into the mold. It is controlled at 680℃ to 750℃ to ensure that the molten metal has enough thermal energy during the flow process so that it can effectively fill the fine structure and complex shape of the mold. Within this temperature range, the viscosity of the molten metal decreases, making it more fluid, which helps to ensure that the molten metal evenly fills the cavity and reduces the generation of air and bubbles.
[0043] Through the low-pressure casting mold, under the influence of the heat capacity of the built-in diverter package, the casting temperature of the water pump housing is controlled between 350℃-450℃. Within this temperature range, it can be ensured that the molten metal reaches appropriate fluidity and solidification speed in the process of filling the cavity, thereby realizing the precise molding of the casting, basically eliminating defects such as cold shut and insufficient pouring of the casting, and can effectively compensate for shrinkage, thereby improving the quality and reliability of the product. At the same time, this temperature range also helps to achieve metal solidification within an appropriate time, ensuring the structural stability and consistency of the casting.
[0044] In some embodiments of the present application, the low-pressure casting method adopts a rapid pressurization crystallization process, which includes: a liquid rising stage, a mold filling stage, a pressurization stage, a pressure holding stage and a pressure relief stage.
[0045] In the liquid raising stage, the molten metal is gradually raised to the casting mold through the low-pressure system to prepare for the subsequent filling. This stage ensures that the molten metal enters the cavity stably and evenly. In the filling stage, the molten metal fills the cavity at a high speed. This stage requires precise control of the flow rate and pressure to ensure that the cavity is fully filled and reduce the possibility of gas inclusions and other defects. The pressurization stage promotes the rapid crystallization of the molten metal by rapidly increasing the pressure, ensuring the formation of a fine and uniform grain structure inside the casting. This process has an important influence on the strength and toughness of the casting. The pressure holding stage maintains a certain pressure to ensure the complete solidification and crystallization of the molten metal, thereby improving the density of the casting and reducing the risk of internal stress and deformation. The pressure relief stage safely releases the pressure inside the cavity through the decompression operation, preparing for the removal of the casting and ensuring the integrity and surface quality of the casting.
[0046] The rapid pressure crystallization process can significantly improve the microstructure of the casting, reduce pores, inclusions and other defects, thereby improving the overall quality and performance of the casting. By optimizing the crystallization process, the process can improve the mechanical properties of the casting, enhance its strength, toughness and corrosion resistance, and meet higher use requirements.
[0047] In some embodiments of the present application, the liquid lifting pressure in the liquid lifting stage is 0.018MPa-0.022MPa, and the liquid lifting time is 2s-4s; and / or the filling pressure in the filling stage is 0.026MPa-0.03MPa, and the filling time is 7s-9s; and / or the boosting pressure in the pressurization stage is 0.033MPa-0.037MPa, and the pressurization time is 1s-3s; and / or the holding pressure in the holding stage is 0.033MPa-0.037MPa, and the holding time is 65s-75s; and / or the pressure relief time in the pressure relief stage is 4s-6s.
[0048] In the liquid raising stage, appropriate liquid raising pressure and time are used to ensure that the metal liquid rises to the cavity stably and evenly, reducing the generation of bubbles. In the filling stage, the filling pressure and time are controlled to ensure that the metal liquid fills the cavity quickly and evenly, thereby improving the filling efficiency of the cavity and the surface quality of the casting. In the pressurization stage, the crystallization process of the metal liquid is accelerated by increasing the pressure, which promotes the formation of a more uniform and delicate grain structure. In the pressure holding stage, the metal liquid is completely solidified by maintaining appropriate pressure and time, improving the density and overall quality of the casting. In the pressure relief stage, the pressure in the cavity is safely released through a reasonable pressure relief time, preparing for the removal of the casting and reducing the risk of deformation.
[0049] An embodiment of the present invention also provides a low-pressure casting mold for a water pump housing. The low-pressure casting mold adopts the low-pressure casting method as described above. The low-pressure casting mold includes: an insert 100, the insert 100 includes an upper mold insert 110 and a lower mold insert 120, the upper mold insert 110 and the lower mold insert 120 cooperate with each other to form a cavity 130; a built-in diverter bag 200, and an inner gate 210 is arranged around the built-in diverter bag 200; a gate sleeve 300, and the gate sleeve 300 is connected to the internal space of the built-in diverter bag 200 to deliver the molten metal from the gate sleeve 300 to the built-in diverter bag 200 and fill the cavity 130.
[0050] like Figure 1 and Figure 2 As shown, the low-pressure casting mold for manufacturing a water pump housing provided in this embodiment has a built-in diverter bag 200 arranged inside the low-pressure casting mold, and the built-in diverter bag 200 is connected with the cavity 130 through an inner gate 210, so that the molten metal in the built-in diverter bag 200 is evenly delivered to the cavity 130, wherein the built-in diverter bag 200 can better fill the defects in the cavity 130 with the molten metal by pressurizing the internal molten metal, thereby improving the quality of the product; and the internal molten metal is emptied by relieving the pressure, thereby improving the process yield. The upper mold insert 110 and the lower mold insert 120 are matched with each other to form a plurality of cavities 130, thereby forming the specific shape of the water pump housing; an inner gate 210 is arranged around the built-in diverter bag 200, so that the molten metal can be guided into the cavity 130 to ensure the smooth progress of the filling process; the gate sleeve 300 is arranged to send the molten metal from the gate sleeve 300 to the built-in diverter bag 200, and finally fill the cavity 130, which is conducive to ensuring that the molten metal is evenly distributed in the cavity 130 to avoid the occurrence of voids or other defects.
[0051] For small aluminum alloy castings, the built-in shunt bag is a new type of low-pressure pouring process. The design of the built-in shunt bag 200 allows the molten metal to be filled into the cavity 130 more smoothly, thereby speeding up the casting process and improving production efficiency; by ensuring uniform filling and flow of the molten metal, the mold helps to reduce defects in the casting and improve the quality of the final product; due to the improvement of production efficiency and optimization of casting quality, the use of the mold provided by this embodiment can reduce production costs and increase the economic benefits of production.
[0052] It should be noted that when casting the water pump housing, at least two exhaust inserts need to be provided on the upper mold insert 110 to ensure that the gas in the cavity 130 is exhausted, so as to ensure that the molten metal is fully filled when filling the mold, thereby reducing the formation of pores or other defects; the exhaust inserts are preferably provided at key positions in the mold, such as on the path of the molten metal flow or in areas where bubbles may appear during the filling process. The lower end surface of the upper mold insert 110 and the upper end surface of the lower mold insert 120 are respectively provided with positioning pins and positioning pin sleeves, and the mutual cooperation of the positioning pins and the positioning pin sleeves enables the upper mold insert 110 and the lower mold insert 120 to play a positioning and guiding role when they are covered.
[0053] In some embodiments of the present application, an annular runner 220 is provided inside the built-in diversion package 200, and the annular runner 220 surrounds and defines a cavity structure.
[0054] like Figure 2 , Figure 4 and Figure 6 As shown, the design of the annular runner 220 means that the molten metal can flow in a continuous annular path, thereby surrounding and defining a central cavity structure, and the cavity structure is conducive to the internal distribution of the built-in diverter bag 200. Among them, the design of the annular runner 220 can make the molten metal liquid enter the mold cavity evenly, thereby achieving more uniform filling and reducing pores and inclusions in the casting; the annular runner 220 can reduce the eddy current generated when the molten metal enters the cavity 130, reduce the possibility of slag mixing, and help maintain the purity of the casting; the annular runner 220 can increase the filling speed of the molten metal, so that it can fill the cavity 130 faster, thereby shortening the production cycle. The formation of the cavity structure provides a basis for the built-in diverter bag 200 to relieve pressure and empty, thereby ensuring that the molten metal of the gate sleeve 300 enters the cavity 130 through the built-in diverter bag 200, and effectively fills the surrounding area of the cavity 130, thereby improving the overall quality of the casting and avoiding defects caused by uneven filling of the molten metal.
[0055] In the low-pressure pouring system, the runner is a channel connecting the riser and the casting gate. It is usually a long strip with a trapezoidal cross-section. After design innovation, it has been improved to form a larger cavity in the mold, connecting the riser and the casting gate, replacing the original runner. Its function and effect are similar to the original low-pressure mold diverter package, but it is different from the original diverter package installed between the mold and the riser. Instead, it is formed in the inner cavity of the mold, so it is called a built-in diverter package.
[0056] In some embodiments of the present application, the built-in diversion bag 200 is provided with a thermal insulation coating; and / or a plurality of heating tubes 140 are provided inside the insert 100; and / or each cavity 130 is correspondingly connected to two inner gates 210.
[0057] like Figure 1 and Figure 2 As shown, the thermal insulation coating in this embodiment is a special coating applied to the surface of the built-in shunt bag 200, and its main function is to provide a thermal insulation effect. The thermal insulation coating can effectively reduce the loss of heat, thereby improving the temperature stability of the built-in shunt bag 200. During the casting process, maintaining a stable temperature is essential to ensure the fluidity and filling of the molten metal; since the thermal insulation coating reduces the conduction and loss of heat, the energy required in the casting process is relatively less, which is conducive to reducing the energy cost of the casting process and improving production efficiency; the thermal insulation coating can keep the surface of the built-in shunt bag 200 at a relatively high temperature, which helps to reduce the solidification and cooling of the molten metal, thereby improving the fluidity and filling of the molten metal; by keeping the surface temperature of the built-in shunt bag 200 stable, the thermal insulation coating can reduce casting defects caused by temperature changes, such as cold cracks, pores and shrinkage defects, which is conducive to improving the quality and reliability of the casting; the thermal insulation coating can reduce the thermal stress and thermal shock on the surface of the built-in shunt bag 200, thereby extending the service life of the built-in shunt bag 200 and reducing the maintenance and replacement costs of the equipment. Preferably, the thermal insulation coating is composed of insulating materials, such as a mixture of ceramic fibers or other thermal insulation materials, which can effectively reduce the conduction and loss of heat.
[0058] like Figure 1 , Figure 3 and Figure 5 As shown, the insert 100 is an important part of the low-pressure casting mold, which is used to contain the molten metal and form the shape of the casting. By designing multiple heating tubes 140 inside the insert 100, the insert 100 and the molten metal are heated, so that the temperature inside the insert 100 reaches the required casting temperature. The heat energy provided by the heating tube 140 can effectively control the temperature of the molten metal, reduce the temperature gradient and thermal stress, thereby reducing the internal defects of the casting and improving the casting quality; compared with the traditional overall heating method, the internal heating tube 140 can more effectively transfer heat energy to the molten metal and the mold, reduce energy waste, and reduce energy costs; reasonable temperature control can reduce the thermal stress and wear of the mold, extend the service life of the mold, reduce replacement costs and production interruptions; stable casting temperature can ensure the consistency of the quality and performance of each casting, and enhance the consistency and reliability of the product.
[0059] like Figure 2As shown, by connecting two ingates 210 to each cavity 130, the molten metal can enter the cavity 130 from two different directions, which helps the molten metal flow in the cavity 130, making the filling more uniform, and can effectively reduce casting defects such as pores and shrinkage holes caused by uneven filling of the molten metal. The provision of two ingates 210 speeds up the filling speed of the molten metal, shortens the entire casting cycle, and is conducive to improving production efficiency, especially in a large-scale production environment, which can significantly increase production; the use of two ingates 210 can also reduce the internal stress caused by uneven temperature caused by the flow of molten metal, and reduce the risk of warping and deformation of the casting; the introduction of molten metal from two different directions helps the structural uniformity of the metal during the solidification process, and improves the mechanical properties and durability of the casting.
[0060] like Figure 7 As shown, the material of the gate sleeve 300 is ceramic material. The ceramic gate sleeve has excellent high temperature resistance and thermal insulation performance, and can withstand the flow of high-temperature molten metal without deformation or cracking. In addition, the surface of the ceramic gate sleeve is smooth and not prone to pores, which can help reduce the occurrence of gas inclusions and prevent the freezing of the inner gate during the pouring process, resulting in the inability to vent and reflux the molten metal when the built-in diverter bag is depressurized.
[0061] In some embodiments of the present application, the thickness of the thermal insulation coating ranges from 3 mm to 3.5 mm.
[0062] like Figure 1 and Figure 2 As shown, by specifying the thickness range of the thermal insulation coating, it is possible to ensure that there is enough thermal insulation layer on the surface of the built-in shunt bag 200 to reduce heat loss. Selecting the appropriate thickness within the specified range can optimize the thermal insulation effect and ensure temperature stability during the casting process. The regulation of the thickness range of the thermal insulation coating can avoid excessive use of materials, thereby saving costs. By ensuring that the coating thickness is within a reasonable range, the material can be used to the maximum extent while meeting the thermal insulation requirements. The selection of the thickness range of the thermal insulation coating may take into account the load bearing capacity of the surface of the built-in shunt bag 200. The appropriate coating thickness can reduce the load on the surface of the built-in shunt bag 200, extend the life of the equipment and reduce maintenance costs. By applying the thermal insulation coating within a suitable thickness range, the efficiency and stability of the casting process can be improved, and the stable temperature helps to maintain the fluidity and quality of the molten metal, thereby improving production efficiency and reducing production interruptions. The appropriate thickness of the thermal insulation coating can ensure that the molten metal maintains a stable temperature when filling the mold, thereby reducing the occurrence of casting defects, which helps to improve the quality and consistency of the casting. Further preferably, the thickness range of the thermal insulation coating is 3.15mm-3.35mm.
[0063] In some embodiments of the present application, the low-pressure casting mold further includes a top plate 400 and a bottom plate 500 , wherein the top plate 400 is disposed on a side close to the upper mold insert 110 , and the bottom plate 500 is disposed on a side close to the lower mold insert 120 .
[0064] like Figure 1 As shown, the top plate 400 and the bottom plate 500 are components of the low-pressure casting mold, the top plate 400 is located on one side of the upper mold insert 110, and the bottom plate 500 is located on one side of the lower mold insert 120. The position and adjustment between the top plate 400 and the bottom plate 500 affect the gap size between the upper mold insert 110 and the lower mold insert 120, thereby controlling the flow and filling of the molten metal during the casting process. Through the adjustment of the top plate 400, the mold gap during the casting process can be accurately controlled, thereby achieving accurate casting of the casting shape and size, which is conducive to improving the quality and consistency of the casting; accurate adjustment can reduce the waste of molten metal and the occurrence of casting defects during the casting process, and by ensuring the appropriate gap between the molds, the leakage and insufficient filling of the molten metal can be reduced, and the scrap rate can be reduced; optimizing the mold adjustment design can reduce production costs, scrap rates and losses caused by production interruptions.
[0065] It should be noted that a push rod is connected between the upper mold insert 110 and the top plate 400 to support the top plate 400; a limit rod, an upper mold connecting column, a spring and a return rod are also provided between the top plate 400 and the upper mold insert 110 to help achieve sustainable production of low-pressure casting molds.
[0066] In this embodiment, the maximum outline size of the water pump housing obtained by casting is required to be 197mm×98mm×58mm, the minimum wall thickness is 3mm, the material is ZL102, and the blank mass is 0.53kg. Due to the high size requirements of the water pump housing, the middle cavity part of the casting needs to be sand cored, and the wall thickness of the casting is small, which makes the casting processability poor and prone to defects such as pores, cold shuts, and insufficient pouring. Therefore, during pouring, there are high requirements for the molten metal temperature and mold temperature, and the filling pressure parameters need to be accurately adjusted.
[0067] like Figure 8 As shown, a solid model with a gating system is made according to the process plan, and the Anycasting software is imported for meshing. The above process parameters are set to obtain the process pressure curve. Among them, the initial pouring temperature is set to 720°C, and a rapid pressurization crystallization process is adopted. The main parameter settings are: the liquid rising pressure is 0.02MPa, and the liquid rising time is 3s; the filling pressure is 0.028MPa, and the filling time is 8s; the boost pressure is 0.035MPa, and the boost time is 2s; the holding crystallization pressure is 0.035MPa, the holding time is 70s, and the pressure relief time is 5s. Mold temperature setting: the upper mold temperature is 350°C, and the lower mold temperature is 450°C.
[0068] Through numerical simulation analysis, the results show that the casting process has no obvious defects in filling, solidification and shrinkage compensation, and the built-in diverter bag can effectively compensate for the shrinkage of the casting, thereby obtaining a good casting. During the pressure holding and solidification process, we found that the casting part of the product was basically solidified in the first 40s, and the remaining time was mainly the solidification of the built-in diverter bag runner part. If we shorten the pressure holding time and release the pressure in advance to 40S, then the built-in diverter bag runner part can be emptied, and the unsolidified aluminum liquid can flow back. In this way, the process yield rate we get will be greatly improved. The yield rate is calculated through three-dimensional simulation. When the middle runner diverter bag is not emptied, it is 54%. According to the ideal state of runner emptying, the process yield rate should be able to reach 75%.
[0069] Fig. 9 This is the low-pressure casting diagram of the water pump housing in this embodiment. Fig.10 Schematic diagram of the ideal state of emptying the low-pressure runner of the water pump housing of this embodiment. Fig.11 This is a solidification simulation analysis diagram of the water pump housing in this embodiment. Fig.12 This is a low-pressure casting product sample of the water pump housing of this embodiment.
[0070] In the simulated production design, by using the built-in diverter bag for pouring, good quality castings can be obtained. Among them, the process yield when the diverter bag is not emptied is 54%. According to the ideal state of the diverter bag being emptied, the process yield is expected to reach 75%. Through numerical simulation analysis, the results show that the pouring process has no obvious defects in filling, solidification and shrinkage feeding. The built-in diverter bag can effectively feed the shrinkage of the casting, thereby obtaining a good casting.
[0071] In actual production, all castings obtained by this low-pressure casting method are qualified. In the initial debugging process of the mold, the emptying state of the middle diverter package after pressure relief was not ideal. Only the middle part was emptied, and the entire diverter package formed a shell. The actual process yield was only about 62%, which failed to meet expectations. In the later production verification process after debugging the mold and adjusting the process parameters, by increasing the thickness of the thermal insulation coating in the built-in diverter package to 3mm-3.5mm, after pouring the 9th-10th mold, the mold temperature rose to 350℃-400℃ under the influence of the heat capacity of the built-in diverter package. The castings basically eliminated defects such as cold shut and insufficient pouring, and could be effectively compensated for shrinkage. At the same time, the diverter package could be emptied to a large extent after pressure relief, and the process yield reached more than 73%. By debugging this process, the expected purpose was finally achieved, the production cost was reduced, and high-quality casting products were obtained, with a mass production qualification rate of more than 87%.
[0072] Table 1 and Table 2 are data comparisons of mechanical properties and process yield of castings obtained by low pressure casting method.
[0073] Table 1 Comparison of mechanical properties of ZL102 single casting bars obtained by low pressure casting and other casting methods Table 2 Comparison of process yield between low pressure casting and other casting methods Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low-pressure casting method for a water pump housing, characterized in that: The low-pressure casting method is applied to a low-pressure casting mold, wherein the low-pressure casting mold includes an upper mold insert, a lower mold insert, a built-in diverter bag and a sprue sleeve. The low-pressure casting method includes: The upper mold insert and the lower mold insert are matched with each other to form a mold cavity; Injecting the molten metal into the built-in diversion package through the sprue sleeve and delivering it to the interior of the built-in diversion package; The molten metal enters along the ingate and fills the cavity.
2. The low pressure casting method according to claim 1, characterized in that When the mold cavity is filled, the built-in diversion package is pressurized to achieve a state in which the molten metal replenishes the mold cavity.
3. The low pressure casting method according to claim 1, characterized in that The initial pouring temperature of the water pump housing is controlled at 680°C-750°C; and / or The casting temperature of the water pump housing is controlled at 350°C-450°C.
4. The low pressure casting method according to claim 1, characterized in that The low-pressure casting method adopts a rapid pressurization crystallization process, which includes: a liquid raising stage, a mold filling stage, a pressurization stage, a pressure holding stage and a pressure relief stage.
5. The low pressure casting method according to claim 4, characterized in that The liquid raising pressure in the liquid raising stage is 0.018MPa-0.022MPa, and the liquid raising time is 2s-4s; and / or The filling pressure in the filling stage is 0.026MPa-0.030MPa, and the filling time is 7s-9s; and / or The boost pressure in the boost stage is 0.033 MPa-0.037 MPa, and the boost time is 1 s-3 s; and / or The holding pressure in the holding stage is 0.033 MPa-0.037 MPa, and the holding time is 65 s-75 s; and / or The pressure relief time in the pressure relief stage is 4s-6s.
6. A low-pressure casting mold for a water pump housing, characterized in that: The low-pressure casting mold adopts the low-pressure casting method according to any one of claims 1 to 5, and the low-pressure casting mold comprises: An insert (100), the insert (100) comprising an upper mold insert (110) and a lower mold insert (120), the upper mold insert (110) and the lower mold insert (120) cooperating with each other to form a mold cavity (130); A built-in diversion package (200), wherein a plurality of inner gates (210) are provided around the built-in diversion package (200); A sprue sleeve (300) is connected to the internal space of the built-in diversion package (200) to deliver molten metal from the sprue sleeve (300) to the built-in diversion package (200) and fill the mold cavity (130).
7. The low pressure casting mold according to claim 6, characterized in that: An annular runner (220) is provided inside the built-in diversion package (200), and the annular runner (220) surrounds and defines a cavity structure.
8. The low pressure casting mold according to claim 6, characterized in that: The built-in diversion package (200) is provided with a thermal insulation coating; and / or A plurality of heating tubes (140) are provided inside the insert (100); and / or Each of the mold cavities (130) is correspondingly connected to two of the inner gates (210).
9. The low-pressure casting mold according to claim 8, characterized in that: The thickness of the thermal insulation coating ranges from 3mm to 3.5mm.
10. The low pressure casting mold according to claim 6, characterized in that: The low-pressure casting mold further comprises a top plate (400) and a bottom plate (500), wherein the top plate (400) is arranged on a side close to the upper mold insert (110), and the bottom plate (500) is arranged on a side close to the lower mold insert (120).
Citation Information
Patent Citations
Low-pressure shunting device
CN109746416A
Casting method and casting device
CN114585462A
Low-pressure casting mold for fluid cover
CN203003120U
Piston low pressure casting device
CN207402088U
Be suitable for low pressure casting die utensil of muffler production
CN207806585U
Cited By
Low-pressure casting mold and casting method for aluminum casting with complex inner cavity
CN119566265A
Modularized low-pressure casting mold
CN120734301A