High-precision and high-flux gradient porous composite material and preparation method thereof

A high-precision, high-flux gradient porous composite material is created by integrating a ceramic layer with a stainless steel matrix, addressing the balance between filtration degree and flux through controlled pore size distribution and sintering, achieving efficient and durable filtration performance.

CN119057067APending Publication Date: 2024-12-03CHANGSHA SHARPEN ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411171747.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing metal porous materials face challenges in achieving a balance between high filtration degree and high filtration flux, particularly in applications requiring high precision and efficiency.

Method used

A high-precision, high-flux gradient porous composite material is developed by synergistically combining a ceramic layer with a porous stainless steel matrix, controlling pore size distribution and thickness, and using a method that includes centrifugal deposition of ceramic slurry on a stainless steel substrate, followed by precise sintering processes.

Benefits of technology

The composite material achieves a relative air permeability coefficient of 5 to 18 m/s and filtration accuracy of 0.15 to 3 μm, with excellent resistance to acid and alkali, high temperature, and stress corrosion, suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057067A_ABST
    Figure CN119057067A_ABST
Patent Text Reader

Abstract

The invention discloses a high-precision and high-flux gradient porous composite material and a preparation method thereof. The preparation method of the composite material comprises the following steps: uniformly mixing stainless steel matrix raw materials including 2205 pre-alloyed powder and a pore-forming agent, placing the mixture in a mold for compression molding to obtain a porous stainless steel green body, and performing primary sintering to obtain a porous stainless steel matrix; uniformly mixing a dispersing agent and a binding agent, adding the high-purity ceramic powder, and fully dispersing to obtain ceramic slurry; the ceramic slurry is uniformly spin-coated and deposited on the inner wall of a porous stainless steel substrate in a high-speed centrifugation manner, and then drying, degreasing treatment and secondary sintering are sequentially performed to obtain the porous stainless steel ceramic. According to the composite material, based on the synergistic effect between the ceramic layer and the stainless steel substrate, the contradiction between high filtration degree and high filtration flux in the filtration process is effectively solved, and tests show that the relative air permeability coefficient of the obtained composite material is 5-18 m < 3 >. M <-2 >. KPa <-1 >. H <-1 >, and the filtration precision is 0.15-3 microns.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a porous composite material, in particular to a high-precision, high-flux gradient porous composite material and a preparation method thereof, and belongs to the field of metal porous material preparation. Background Art

[0002] Metal porous materials have the advantages of both structural materials and porous materials. They have the advantages of low density, high specific strength, large specific surface area, high temperature resistance, corrosion resistance, sound insulation, heat insulation and high permeability. They have developed into a new type of structural functional material, showing broad application prospects in many fields such as aerospace, chemical industry, building materials, metallurgy, petrochemical, machinery, medicine and environmental protection. With the vigorous development of industry, more typical application scenarios and usage requirements are constantly being proposed, and the materials, preparation methods, material structure design and other aspects of porous materials have also made great progress. Thanks to the special properties of metal porous materials, they have attracted more and more attention and become an important part of the field of materials science, and are constantly developing in the direction of high performance, long life and low cost.

[0003] There are a wide variety of metal porous materials, which can be subdivided into hundreds of categories such as gold, silver, copper, nickel, aluminum, magnesium, titanium, chromium, molybdenum, tungsten, stainless steel, iron-based alloys, nickel-based alloys, Hastelloy alloys, intermetallic compounds, etc. According to their materials, stainless steel porous materials stand out due to their high corrosion resistance, high specific strength and economy, and become the most widely used type of metal porous materials, especially 316L stainless steel porous materials. Compared with austenitic stainless steel, duplex stainless steel has excellent mechanical properties and corrosion resistance due to its ferrite and austenite dual-phase structure. As a typical grade of the second-generation duplex stainless steel, 2205 stainless steel has higher strength, corrosion resistance and weldability, especially its outstanding pitting resistance in halogen ion environments. In addition, due to the proprietary application field and the high threshold of production technology, duplex stainless steel products have always maintained a high economic value. As a resource-saving high-performance stainless steel, the production and application of duplex stainless steel are more in line with the future development direction of stainless steel, especially in the context of the current large-scale consumption of nickel resources in the new energy field. To this end, the development of duplex stainless steel porous materials is more in line with the current development trend of high performance and low cost of metal porous materials.

[0004] In recent years, the demand for high-precision and high-efficiency sintered metal porous materials in industries such as petrochemicals, electricity, pharmaceuticals and energy has continued to increase. Summary of the invention

[0005] In view of the problems of the prior art, the first object of the present invention is to provide a high-precision, high-flux gradient porous composite material. The porous composite material is based on the synergistic effect between the ceramic layer and the porous stainless steel matrix, and by constructing a gradient porous channel, it effectively solves the contradiction between high filtration degree and high filtration flux in the filtration process. By strictly controlling the pore size distribution between the ceramic layer and the matrix layer and the thickness of the ceramic layer, a relative air permeability coefficient of 5 to 18 m / s is obtained. 3 ·m -2 kPa -1 ·h -1 , composite material with a filtration accuracy of 0.15~3μm.

[0006] The second object of the present invention is to provide a method for preparing a high-precision, high-throughput gradient porous composite material. The method controls the mass ratio between the components of the raw materials, first obtains a porous stainless steel matrix, then centrifugally deposits the ceramic slurry on the stainless steel surface, and through the complementary advantages of the porous stainless steel matrix layer and the ceramic layer, obtains an asymmetric porous material that is resistant to acid and alkali, high temperature, stress corrosion, and has high filtration accuracy and efficiency; the method has the advantages of stable process, high efficiency and low cost, and is suitable for large-scale industrial preparation.

[0007] In order to achieve the above technical objectives, the present invention provides a method for preparing a high-precision, high-throughput gradient porous composite material, comprising:

[0008] 1) mixing stainless steel matrix raw materials including 2205 pre-alloyed powder and pore-forming agent uniformly and placing them in a mold for pressing to obtain a porous stainless steel green body, and then sintering them once to obtain a porous stainless steel matrix;

[0009] 2) After the dispersant and the binder are evenly mixed, high-purity ceramic powder is added and fully dispersed to obtain a ceramic slurry;

[0010] 3) The ceramic slurry is evenly spin-coated and deposited on the inner wall of the porous stainless steel substrate by high-speed centrifugation, and then dried, degreased and sintered twice in sequence to obtain;

[0011] The 2205 pre-alloyed powder includes 10-30% pre-alloyed powder with a particle size of 18-23 μm and 70-90% pre-alloyed powder with a particle size of 48-75 μm;

[0012] The particle size of the ceramic powder is 0.5 to 15 μm.

[0013] As a preferred solution, the amount of pore former added to the stainless steel matrix raw material is 2-10% of the total mass of the raw material.

[0014] As a preferred solution, the pore-forming agent is K 2 SO4 .

[0015] As a preferred solution, the compression molding process is: cold isostatic pressing is adopted at a pressure of 80 to 200 MPa for 3 to 10 minutes.

[0016] As a preferred solution, the conditions for the primary sintering are: heating to 1150-1250° C. at a heating rate of 1-3° C. / min and sintering for 1-3 hours.

[0017] As a preferred solution, the dispersant is polyethylene glycol.

[0018] As a preferred solution, the binder is at least one of polyvinyl alcohol (PVA), polyvinyl butyral (PVB), methyl cellulose (MC) and phenolic resin.

[0019] As a preferred solution, in the ceramic slurry, the mass proportion of the dispersant is 2-10%, the mass proportion of the binder is 3-15%, and the mass proportion of the high-purity ceramic powder is 10-30%.

[0020] As a preferred solution, the purity of the high-purity ceramic powder is ≥99.9%.

[0021] As a preferred solution, the high-purity ceramic powder is Al 2 O 3 、SiO 2 、ZrO 2 and TiO 2 At least one of .

[0022] As a preferred solution, the particle size of the high-purity ceramic powder is 0.5-15 μm.

[0023] As a preferred solution, the conditions for high-speed centrifugation are: a rotation speed of 100 to 10,000 r / min and a time of 10 to 30 min.

[0024] As a preferred solution, the degreasing process is: adopting a three-stage heating method, the first-level temperature platform is 230-270°C, the second-level temperature platform is 280-320°C, and the third-level temperature platform is 380-420°C. The insulation time of each temperature platform is 2-5h, and the heating rate is 1-2°C / min.

[0025] As a preferred solution, the secondary sintering process is: in a protective atmosphere, heating to 700-1000°C at 1-3°C / min, keeping the temperature for 1-3h, and then cooling to room temperature with the furnace.

[0026] The present invention also provides a high-precision, high-flux gradient porous composite material, which is prepared by any one of the preparation methods described above; the thickness of the ceramic layer in the composite material is 30 to 40 μm, and the relative air permeability is 5 to 18 μm. 3 ·m -2 kPa -1 ·h -1 The filtration accuracy is 0.15~3μm.

[0027] Compared with the prior art, the beneficial technical effects of the technical solution of the present invention are:

[0028] 1) The porous composite material provided by the present invention is based on the synergistic effect between the ceramic layer and the porous stainless steel matrix, and effectively solves the contradiction between high filtration degree and high filtration flux in the filtration process by constructing a gradient porous channel. Among them, by strictly controlling the pore size distribution between the ceramic layer and the matrix layer and the thickness of the ceramic layer, a relative air permeability coefficient of 5 to 18 m / s is obtained. 3 ·m -2 kPa -1 ·h -1 , composite material with a filtration accuracy of 0.15~3μm.

[0029] 2) The preparation method provided by the present invention controls the mass ratio between the components of the raw materials, first obtains a porous stainless steel matrix, and then centrifugally deposits the ceramic slurry on the stainless steel surface. Through the complementary advantages of the porous stainless steel matrix layer and the ceramic layer, an asymmetric porous material with acid and alkali resistance, high temperature resistance, stress corrosion resistance, high filtration accuracy and efficiency is obtained; this method has the advantages of stable process, high efficiency and low cost, and is suitable for large-scale industrial preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the cold isostatic pressing die structure of the present invention;

[0031] Among them, 1. core rod; 2. rubber sleeve; 3. annular rubber plug; 4. annular stainless steel plug; 5. clamp; 6. stainless steel powder

[0032] Figure 2 This is a schematic diagram of the structure of a molding device using centrifugal deposition of ceramic slurry in the present invention;

[0033] Among them, 1. motor; 2. chuck; 3. rubber plug; 4. porous stainless steel substrate; 5. ceramic layer; 6. dispersion; 7. dispersion collecting cover; 8. fastening screws; 9. bearing. DETAILED DESCRIPTION

[0034] The present invention will be further described below in combination with specific examples based on the technical solution of the present invention, but the protection scope of the present invention is not limited to the following embodiments.

[0035] Example 1

[0036] A ceramic-stainless steel composite gradient porous material is prepared, and the preparation method thereof is as follows:

[0037] 1) Weigh the powders according to the mass fractions: 20wt% 2205 stainless steel pre-alloyed powder (18-23μm), 80wt% 2205 stainless steel pre-alloyed powder (48-75μm). Then add 5% K 2 SO 4 , use a V-type mixer to mix evenly for 48 hours. Figure 1 As shown in the figure, the pressing mold is assembled: the molding mold consists of a thin-walled core rod, a rubber sleeve, an annular rubber plug and an annular stainless steel plug; then, the evenly mixed powder is evenly filled into the mold cavity between the outer rubber sleeve and the core rod, and the mold is sealed by the annular rubber plug and the annular stainless steel plug in conjunction with the rubber sleeve. Then, an outer clamp is used to further seal and waterproof the contact area between the rubber sleeve and the annular rubber plug. The sealed and water-proof mold is placed in a cold isostatic press for pressing, with a pressing pressure of 150MPa and a holding time of 5 minutes. Finally, after the pressing is completed, loosen the clamp, take out the annular stainless steel plug and the rubber plug, and remove the outer rubber sleeve to obtain the pressed 2205 porous stainless steel green body.

[0038] 2) The porous stainless steel green body obtained in step (1) is sintered according to the set program. The porous stainless steel sintered green body is placed vertically in an alumina crucible. When the temperature is lower than 1000°C, vacuum sintering is adopted, and the heating rate is 2°C / min. When the temperature is higher than 1000°C, N 2 Atmosphere partial pressure sintering, the gas pressure in the furnace is 800-1000Pa, the heating rate is 1℃ / min. The final sintering temperature is 1200℃, and the holding time is 2 hours. Then the sintered stainless steel porous blank is washed with water to completely remove the residual pore-forming agent to obtain the 2205 porous stainless steel matrix.

[0039] 3) Prepare a solution with anhydrous ethanol according to the mass fractions: dispersant accounts for 4% by mass, binder accounts for 6% by mass, and then weigh 20% of the solution by mass of ZrO 2 The powder and the solution are fully stirred and mixed to obtain a ceramic slurry. Among them, the dispersant is polyethylene glycol (PEG), the binder is polyvinyl butyral (PVB), and ZrO 2 The particle size distribution of the powder is 1 to 2 μm.

[0040] 4) The open end of the sintered porous stainless steel billet is sealed with a rubber plug, and then an appropriate amount of ZrO obtained in step (3) is poured into the 2 The ceramic slurry is poured into the 2205 porous stainless steel billet, and the porous stainless steel billet is Figure 2The horizontal connection shown is fixed to the centrifuge, and the centrifugal speed and time are set to 5000r / min and 20 minutes respectively. The ceramic slurry ZrO 2 The ceramic layer is evenly centrifugally deposited on the inner wall of the porous stainless steel billet. After the inner ceramic layer is centrifugally coated, the stainless steel billet is transferred to a vacuum oven and dried under negative pressure at 80°C for 2 hours to completely remove the anhydrous ethanol.

[0041] 5) The ZrO coated 2 The ceramic layer porous stainless steel billet is transferred to the sintering furnace, and degrease is carried out in an argon atmosphere at low temperature. Three insulation platforms are set at 250℃, 300℃ and 400℃, respectively, with a heating rate of 2℃ / min and a insulation time of 4 hours. After completely removing the dispersant, sintering is carried out in a nitrogen atmosphere, with an air pressure of 800-1000Pa in the furnace, a maximum sintering temperature of 700℃, a heating rate of 2℃ / min, and a insulation time of 2 hours. After high-temperature sintering and cooling, ZrO is obtained. 2 Ceramic-2205 stainless steel composite gradient porous material.

[0042] After testing, the ZrO prepared above 2 ZrO2 in ceramic-2205 stainless steel composite gradient porous material 2 The thickness of the ceramic layer is 39 μm, and the relative air permeability coefficient of the gradient porous material is 8.32 m 3 ·m -2 kPa -1 ·h -1 , and its filtration accuracy is 0.28μm.

[0043] Example 2

[0044] The difference between Example 2 and Example 1 is that Al 2 O 3 Powder replaces ZrO 2 Powder, while Al 2 O 3 The powder particle size is 14 μm. The preparation process of Example 2 is the same as that of Example 1, except that Example 2 is coated with Al 2 O 3 The highest sintering temperature of the ceramic layer porous stainless steel billet is 1000℃. After high temperature sintering, Al 2 O 3 Ceramic-2205 stainless steel composite gradient porous material. After testing, the Al 2 O 3 The thickness of the ceramic layer of the ceramic-2205 stainless steel composite gradient porous material is 37 μm, and the relative air permeability coefficient of the gradient porous material is 16.35 m 3 ·m -2 kPa -1 ·h-1 , and its filtration accuracy is 2.7μm. When using different types of ceramic powders and powders with coarser particle sizes, higher sintering temperatures should be used to achieve good metallurgical bonding between ceramic particles due to the poor sintering activity of the powders.

[0045] Example 3

[0046] Compared with Example 1, Example 3 uses exactly the same ceramic powder and composition, the only difference is that Example 3 is coated with ZrO 2 The highest sintering temperature of the ceramic layer porous stainless steel billet is 900℃. After high temperature sintering, ZrO 2 Ceramic-2205 stainless steel composite gradient porous material. After testing, the ZrO 2 ZrO2 in ceramic-2205 stainless steel composite gradient porous material 2 The thickness of the ceramic layer is 38 μm, and the relative air permeability coefficient of the gradient porous material is 5.86 m 3 ·m -2 kPa -1 ·h -1 , and its filtration accuracy is 0.2μm. When finer powder raw materials are sintered at a higher temperature, the ceramic layer will be further densified. As the sintering temperature increases, ZrO 2 The sintering necks between the membrane particles are formed and grow, the relative air permeability coefficient gradually decreases, and the average pore size gradually decreases. Controlling the sintering temperature according to the particle size of the powder can better ensure a better match between the filtration accuracy and the air permeability.

[0047] Example 4

[0048] Compared with Example 1, Example 4 uses exactly the same ceramic powder and component composition, the only difference is that K is not added during the preparation process of the porous 2205 ceramic matrix in Example 4. 2 SO 4 Pore-forming agent, ZrO is prepared after high temperature sintering 2 Ceramic-2205 stainless steel composite gradient porous material. After testing, the ZrO 2 ZrO2 in ceramic-2205 stainless steel composite gradient porous material 2 The thickness of the ceramic layer is 39 μm, and the relative air permeability coefficient of the gradient porous material is 7.69 μm. 3 ·m -2 kPa -1 ·h -1 , and its filtration accuracy is 0.27μm. When the porous stainless steel matrix is ​​prepared without adding a placeholder pore-forming agent, the prepared ZrO 2The relative air permeability coefficient of the ceramic-2205 stainless steel composite gradient porous material will decrease slightly, which is caused by the decrease in the porosity of the stainless steel matrix. In order to prepare composite gradient porous materials with better performance, it is important to use pore-forming agents to obtain a stainless steel matrix with higher porosity.

[0049] Example 5

[0050] Compared with Example 1, Example 5 uses exactly the same ceramic powder and component composition, the only difference is that the centrifugal deposition time of the ceramic slurry in Example 5 is extended to 30 minutes, and ZrO is prepared after high-temperature sintering. 2 Ceramic-2205 stainless steel composite gradient porous material. After testing, the ZrO 2 ZrO2 in ceramic-2205 stainless steel composite gradient porous material 2 The thickness of the ceramic layer is 38 μm, and the relative air permeability coefficient of the gradient porous material is 6.82 m 3 ·m -2 kPa -1 ·h -1 , and its filtration accuracy is 0.23μm. During the centrifugal deposition of ceramic slurry, with the increase of centrifugal speed and time, the coarse-grained ceramic particles tend to approach the porous stainless steel matrix under the action of centrifugal force, while a higher proportion of fine powder is left on the inner wall of the ceramic slurry. During high-temperature densification, the sintering driving force of fine powder is greater, and the inner wall of the ceramic layer obtains a higher densification, which causes a slight decrease in the relative permeability coefficient of the composite gradient porous material.

[0051] Comparative Example 1

[0052] Comparative Example 1 uses the same ceramic powder and composition as Example 1, except that ZrO is coated on the surface of the ceramic powder. 2 The sintering process of the ceramic layer porous stainless steel billet shortened the three degreasing and heat preservation platform times at 250℃, 300℃ and 400℃ to 1 hour, and the heating rate was increased to 5℃ / min. ZrO was prepared after high temperature sintering. 2 Ceramic-2205 stainless steel composite gradient porous material. It was found that ZrO 2 There are obvious cracks and bubbles on the surface of the ceramic layer. 2 Ceramic-2205 stainless steel composite gradient porous materials cannot meet the needs of precision filtration. The thermal expansion coefficients of the ceramic layer and the stainless steel substrate layer in the ceramic-stainless steel composite gradient porous material are quite different, and the sintering preparation process must use a slower heating rate to avoid cracking of the ceramic layer. In addition, the sintering process of powder metallurgy products must ensure that the dispersant and forming agent are completely removed.

[0053] Comparative Example 2

[0054] The difference between Comparative Example 2 and Example 2 is that the amount of ceramic slurry added in Comparative Example 2 is only one-fourth of that in Example 2. Al 2 O 3 Ceramic-2205 stainless steel composite gradient porous material. After testing, the Al 2 O 3 The thickness of the ceramic layer of the ceramic-2205 stainless steel composite gradient porous material is 9 μm, and the relative air permeability coefficient of the gradient porous material is 21.45 m 3 ·m -2 kPa -1 ·h -1 , and its filtration accuracy is 3.2μm. When adding less ceramic slurry during centrifugal deposition, an ultra-thin ceramic layer can be prepared. At the same time, as the thickness of the ceramic layer decreases, the relative air permeability coefficient of the gradient porous material can be increased to a certain extent. However, at this time, the strength of the ultra-thin ceramic layer is seriously insufficient. In actual filtration, the ceramic layer of the gradient porous material is very easy to crack and fail under large flow rates.

[0055] Comparative Example 3

[0056] Comparative Example 3 uses the same ceramic powder and composition as Example 1, except that ZrO 2 The highest sintering temperature of the ceramic layer porous stainless steel billet is 1100℃. After high temperature sintering, ZrO 2 Ceramic-2205 stainless steel composite gradient porous material. After testing, the ZrO 2 ZrO2 in ceramic-2205 stainless steel composite gradient porous material 2 The thickness of the ceramic layer is 36 μm, and the relative air permeability coefficient of the gradient porous material is 1.03 m 3 ·m -2 kPa -1 ·h -1 , and its filtration accuracy is 0.1μm. When the ceramic layer is sintered, a suitable sintering temperature needs to be adopted. When the sintering temperature is too high, it is easy to greatly reduce the porosity in the ceramic layer, thereby greatly reducing the filtration efficiency.

[0057] Comparative Example 4

[0058] Comparative Example 4 uses the same ceramic powder and composition as Example 1, except that the 0.2 μm ultrafine ZrO 2 Ceramic powder, after high temperature sintering, is prepared to obtain ZrO 2 Ceramic-2205 stainless steel composite gradient porous material. After testing, the ZrO 2ZrO2 in ceramic-2205 stainless steel composite gradient porous material 2 The thickness of the ceramic layer is 34 μm, and the relative air permeability coefficient of the gradient porous material is 1.14 m 3 ·m -2 kPa -1 ·h -1 , and its filtration accuracy is 0.13μm. Ultrafine ceramic powder has a high specific surface area and high sintering activity. The densification driving force of the sintering process is large, which makes the sintering preparation window of its porous materials narrow, and it is difficult to prepare composite gradient porous materials with high filtration flux and high filtration accuracy.

[0059] Comparative Example 5

[0060] Compared with Example 1, Comparative Example 5 uses exactly the same ceramic powder and component composition, the only difference is that when preparing the 2205 porous stainless steel substrate of Comparative Example 5, only 2205 stainless steel pre-alloyed powder with a single particle size range (18-23μm or 48-75μm) is used. During the implementation of Comparative Example 5, it was found that when only stainless steel pre-alloyed powder with a single particle size range was used, the pressed green sheet was very easy to crack and difficult to form during the pressing process. When powders with two particle size ranges (18-23μm and 48-75μm) were uniformly mixed, the formability was greatly improved. Although the addition of forming agents such as paraffin, PEG and polyethylene glycol to single particle size powder can assist in molding, the inevitable introduction of sintering and degreasing process greatly reduces the preparation efficiency of the porous stainless steel substrate.

Claims

1. A method for preparing a high-precision, high-throughput gradient porous composite material, characterized in that: include: 1) mixing stainless steel matrix raw materials including 2205 pre-alloyed powder and pore-forming agent uniformly and placing them in a mold for pressing to obtain a porous stainless steel green body, and then sintering them once to obtain a porous stainless steel matrix; 2) After the dispersant and the binder are evenly mixed, high-purity ceramic powder is added and fully dispersed to obtain a ceramic slurry; 3) The ceramic slurry is evenly spin-coated and deposited on the inner wall of the porous stainless steel substrate by high-speed centrifugation, and then dried, degreased and sintered twice in sequence to obtain; The 2205 pre-alloyed powder includes 10-30% pre-alloyed powder with a particle size of 18-23 μm and 70-90% pre-alloyed powder with a particle size of 48-75 μm; The particle size of the ceramic powder is 0.5 to 15 μm.

2. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: The amount of the pore-forming agent added to the stainless steel matrix raw material is 2-10% of the total mass of the raw material; the pore-forming agent is K2SO4 with a particle size of 30-60 μm.

3. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: The pressing process is: cold isostatic pressing is adopted, at a pressure of 80 to 200 MPa, and the pressure is maintained for 3 to 10 minutes.

4. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: The conditions of the primary sintering are: heating to 1150-1250° C. at a heating rate of 1-3° C. / min and sintering for 1-3 hours.

5. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: The dispersant is polyethylene glycol; the binder is at least one of polyvinyl alcohol (PVA), polyvinyl butyral (PVB), methyl cellulose (MC) and phenolic resin.

6. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: In the ceramic slurry, the mass proportion of the dispersant is 2-10%, the mass proportion of the binder is 3-15%, and the mass proportion of the high-purity ceramic powder is 10-30%.

7. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: The purity of the high-purity ceramic powder is ≥99.9%; the high-purity ceramic powder is at least one of Al2O3, SiO2, ZrO2 and TiO2; the particle size of the high-purity ceramic powder is 0.5 to 15 μm.

8. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: The conditions of the high-speed centrifugation are: a rotation speed of 100 to 10,000 r / min and a time of 10 to 30 min; the process of the degreasing treatment is: a three-stage heating method is adopted, the first-stage temperature platform is 230 to 270°C, the second-stage temperature platform is 280 to 320°C, and the third-stage temperature platform is 380 to 420°C. The insulation time of each temperature platform is 2 to 5 hours, and the heating rate is 1 to 2°C / min.

9. The method for preparing a high-precision, high-throughput gradient porous composite material according to claim 1, characterized in that: The secondary sintering process is: in a protective atmosphere, heating to 700-1000° C. at 1-3° C. / min, keeping the temperature for 1-3 hours, and then cooling to room temperature along with the furnace.

10. A high-precision, high-throughput gradient porous composite material, characterized in that: The composite material is prepared by the preparation method according to any one of claims 1 to 9; the thickness of the ceramic layer in the composite material is 30 to 40 μm, and the relative air permeability is 5 to 18 μm. 3 ·m -2 kPa -1 ·h -1 The filtration accuracy is 0.15~3μm.