Preparation method of network interlayer assisted brazing Cf / SiC / Nb corrosion-resistant joint

By introducing a foam nickel intermediate layer into the brazing of Cf/SiC ceramic matrix composite material and Nb, a three-dimensional network structure is formed, which solves the stress and galvanic corrosion problems of the brazed joint in humid environments, and significantly improves the corrosion resistance and Shear strength, suitable for high-temperature strength brazed joint design.

CN119057167APending Publication Date: 2024-12-03HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411285263.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The brazed joints of Cf/SiC ceramic matrix composite materials and high-temperature metal Nb are prone to stress corrosion and galvanic corrosion failure in humid environments, resulting in poor corrosion resistance and affecting the reliability of missile engines, military satellites and rocket engines.

Method used

Using nickel foam as the intermediate layer auxiliary brazing, the Cf/SiC ceramic matrix composite material, Nb and TiNiNb foil is processed in a vacuum environment to form a structure of Cf/SiC/TiNiNb/foam nickel foam/TiNiNb/main material Nb, and the structure of Nb is formed in the vacuum environment. Vacuum brazing is made at 1100℃~1250℃ to generate a three-dimensional network structure to improve the corrosion resistance of the joint.

Benefits of technology

The room temperature shear strength and corrosion resistance of the joints are significantly improved. The corrosion area of ​​the foam nickel-assisted brazed joint is much lower than that of the joint without intermediate layer, and is simple to process, low price, and universal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057167A_ABST
    Figure CN119057167A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a Cf / SiC / Nb corrosion-resistant joint, in particular to a preparation method of a network interlayer auxiliary brazing Cf / SiC / Nb corrosion-resistant joint. The problem that an existing Cf / SiC and Nb brazed joint is poor in corrosion resistance is solved. The preparation method comprises the following steps: 1, dipping foamed nickel in diluted hydrochloric acid for treatment; secondly, assembling is conducted according to the structure of base metal Cf / SiC / TiNiNb / foamed nickel / TiNiNb / base metal Nb; and 3, brazing. The method is used for preparing the network interlayer auxiliary brazing Cf / SiC / Nb anti-corrosion joint.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to C f Preparation method of / SiC / Nb corrosion-resistant joint. Background Art

[0002] C f As a new type of strategic material, SiC ceramic matrix composites have broad application prospects in the manufacture of missile engines, military satellites, military aircraft, rocket engines, etc. Due to its poor processability, it is often necessary to connect with metal materials to form complex components to meet practical application needs. In particular, for the new generation of attitude control engines, large-size C f The connection between the nozzle and the thrust chamber made of high-temperature alloy is a key link in its manufacturing process. The high-temperature alloy can usually be made of Nb metal with excellent processing performance and high-temperature strength. f There are two main ways to connect the SiC ceramic matrix composite nozzle and the metal Nb thrust chamber: mechanical connection through flanges and direct welding. Among them, the mechanical connection method is not conducive to engine weight reduction, and the flexible graphite sealing gasket used is prone to failure during long-term engine operation, which seriously reduces the reliability of engine operation. The brazing connection method can overcome the above problems and become an ideal connection method to give full play to the performance advantages of ceramic matrix composite nozzles and reduce system weight.

[0003] However, C f Due to the differences in material composition and chemical properties of the parent materials and the existence of residual stress, the brazed components of SiC / SiC ceramic matrix composites and high-temperature metal Nb dissimilar materials face serious corrosion failure risks during storage and service in the humid environment of Hainan. The main reasons are as follows: (1) The elastic modulus and thermal expansion coefficient of ceramic matrix composites are quite different from those of metals. Therefore, ceramic matrix composites and metal joints are prone to generate high thermal stress during the brazing process and engine service, which in turn induces stress corrosion failure under the erosion of corrosive media. (2) C f The difference in chemical composition between / SiC ceramic matrix composites and Nb leads to a large difference in the intrinsic corrosion potential of the materials, which is very likely to cause galvanic corrosion. (3) The South China Sea is a typical marine atmospheric environment, and the material corrosion problem is very prominent in its high salt fog natural environment. Therefore, by developing C f The new brazing technology of / SiC ceramic-based composite materials and Nb, which also has excellent high-temperature strength, can achieve corrosion protection of brazed joints, which is of great significance to the storage and service of missile engines, military satellites, military aircraft, and rocket engine equipment in Hainan and the South China Sea. Summary of the invention

[0004] The present invention aims to solve the existing C f / SiC and Nb brazing joints have poor corrosion resistance, and thus provide a network intermediate layer to assist brazing C f Preparation method of / SiC / Nb corrosion-resistant joint.

[0005] A network intermediate layer auxiliary brazing C f The preparation method of the / SiC / Nb corrosion resistant joint is carried out according to the following steps:

[0006] 1. Immersing the nickel foam in dilute hydrochloric acid, then washing and drying, to obtain the acid-treated nickel foam;

[0007] 2. C f / SiC ceramic matrix composites, Nb, TiNiNb foils and acid-treated nickel foams were prepared according to the parent material C f / SiC / TiNiNb / foam nickel / TiNiNb / parent material Nb structure is assembled to obtain an assembled component;

[0008] 3. Place the assembled components in a vacuum brazing furnace, keep them warm for 5-15 minutes under vacuum environment and temperature of 1100-1250°C, then cool them down to below 100°C and take out the welded parts to obtain the network intermediate layer auxiliary brazing C f / SiC / Nb corrosion resistant joint.

[0009] The beneficial effects of the present invention are:

[0010] The present invention introduces a foam nickel intermediate layer to assist brazing C f / SiC ceramic matrix composite material and Nb metal form a good joint. This method can introduce a three-dimensional network structure into the weld and add Ni with good corrosion resistance, which can significantly promote the homogenization of the joint structure, that is, prevent the large-scale enrichment and continuous distribution of brittle and hard phases and non-corrosion-resistant phases from forming weak links. At the same time, a large amount of in-situ generated TiNi phases and uniformly distributed solid solution phases Nb (s, s) both show good mechanical and corrosion-resistant strengthening effects. The C f / SiC-Nb good corrosion-resistant joint has a room temperature shear strength of 125.78MPa, which is 3.7 times that of the brazed joint without an intermediate layer; the corrosion area of ​​the foam nickel assisted brazed joint after 28 days of accelerated corrosion test is much lower than that of the joint without an intermediate layer.

[0011] 1. The processing method of the present invention is simple and inexpensive, and the preparation and assembly of the base material, the solder, and the intermediate layer can be achieved through only basic mechanical processing and pre-treatment.

[0012] 2. The present invention utilizes three-dimensional network nickel foam as the brazing intermediate layer to introduce a network structure into the joint, while improving the brazing seam component design, effectively alleviating the stress concentration of the joint, improving the mechanical properties of the joint, and enhancing its corrosion resistance.

[0013] 3. The present invention can also be extended to other brazing joint structure designs that require enhanced corrosion resistance, and the invention has universal applicability.

[0014] Instruction Manual

[0015] Figure 1 The network intermediate layer auxiliary brazing C prepared in Example 1 f Microstructure of the / SiC / Nb corrosion-resistant joint, A is the TiNi phase, B is the Nb(s,s) phase;

[0016] Figure 2 C brazed without intermediate layer prepared for comparative experiment f Microstructure of the / SiC / Nb joint, A is the brittle phase Ti (Nb, Ni);

[0017] Figure 3 The network intermediate layer auxiliary brazing C prepared in Example 1 f / SiC / Nb corrosion resistant joints and comparative experiments on C brazed joints without intermediate layer f Corrosion morphology of the joints of SiC / Nb joints after immersion accelerated corrosion test in 15wt.% NaCl solution at room temperature for 28 days, (a) is a comparative experiment, (b) is Example 1;

[0018] Figure 4 The network intermediate layer auxiliary brazing C prepared in Example 1 f / SiC / Nb corrosion resistant joints and comparative experiments on C brazed joints without intermediate layer f The shear strength time-varying curves of the joints of SiC / Nb were respectively subjected to an accelerated corrosion test after being immersed in a 15wt.% NaCl solution at room temperature for 28 days. (a) is a comparative experiment, and (b) is Example 1. DETAILED DESCRIPTION

[0019] Specific implementation method 1: This implementation method is a network intermediate layer auxiliary brazing C f The preparation method of the / SiC / Nb corrosion resistant joint is carried out according to the following steps:

[0020] 1. Immersing the nickel foam in dilute hydrochloric acid, then washing and drying, to obtain the acid-treated nickel foam;

[0021] 2. C f / SiC ceramic matrix composites, Nb, TiNiNb foils and acid-treated nickel foams were prepared according to the parent material C f / SiC / TiNiNb / foam nickel / TiNiNb / parent material Nb structure is assembled to obtain an assembled component;

[0022] 3. Place the assembled components in a vacuum brazing furnace, keep them warm for 5-15 minutes under vacuum environment and temperature of 1100-1250°C, then cool them down to below 100°C and take out the welded parts to obtain the network intermediate layer auxiliary brazing C f / SiC / Nb corrosion resistant joint.

[0023] The beneficial effects of this embodiment are:

[0024] In this embodiment, a foam nickel intermediate layer is introduced to assist the brazing of C f / SiC ceramic matrix composite material and Nb metal form a good joint. This method can introduce a three-dimensional network structure into the weld and add Ni with good corrosion resistance, which can significantly promote the homogenization of the joint structure, that is, prevent the large-scale enrichment and continuous distribution of brittle and hard phases and non-corrosion-resistant phases to form weak links. At the same time, a large amount of in-situ generated TiNi phases and uniformly distributed solid solution phases Nb (s, s) both show good mechanical and corrosion-resistant strengthening effects. The C f / SiC-Nb good corrosion-resistant joint has a room temperature shear strength of 125.78MPa, which is 3.7 times that of the brazed joint without an intermediate layer; the corrosion area of ​​the foam nickel assisted brazed joint after 28 days of accelerated corrosion test is much lower than that of the joint without an intermediate layer.

[0025] 1. The processing method of this embodiment is simple and low-cost, and the preparation and assembly of the base material, the brazing material, and the intermediate layer can be achieved through only basic mechanical processing and pre-treatment.

[0026] 2. This embodiment uses three-dimensional network nickel foam as the brazing intermediate layer to introduce a network structure into the joint, while improving the brazing seam component design, effectively alleviating the stress concentration of the joint, improving the mechanical properties of the joint, and enhancing its corrosion resistance.

[0027] 3. This embodiment can also be extended to other brazing joint structure designs that require enhanced corrosion resistance, and the invention has universal applicability.

[0028] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that the pore diameter of the nickel foam described in step 1 is 100 μm to 200 μm, the porosity is 30% to 70%, and the thickness is 1 mm to 4 mm. Other aspects are the same as specific implementation method 1.

[0029] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: in step 1, the nickel foam is immersed in 3.5% to 25% by mass dilute hydrochloric acid for 5 to 15 minutes at room temperature and pressure. The rest is the same as specific implementation method 1 or 2.

[0030] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the atomic content ratio of Ti to Ni in the TiNiNb foil described in step 2 is 1:1, and the atomic percentage content of Nb is 5% to 15%; the thickness of the TiNiNb foil described in step 2 is 0.1 mm to 0.5 mm. Others are the same as specific embodiments 1 to 3.

[0031] Specific implementation method 5: This implementation method is different from the specific implementation methods 1 to 4 in that: the C in step 2 f The C / SiC ceramic matrix composite material is pretreated f / SiC ceramic matrix composite material, and the pretreatment is specifically carried out in the following steps: C f The surface to be welded of the SiC ceramic matrix composite material is polished with 300# gold sandpaper, 600# metallographic sandpaper and 1000# metallographic sandpaper in sequence, then ultrasonically cleaned in anhydrous ethanol, and finally dried. The rest is the same as the specific embodiments 1 to 4.

[0032] Specific embodiment 6: This embodiment is different from specific embodiments 1 to 5 in that: the Nb described in step 2 is pre-treated Nb, and the pre-treatment is specifically performed according to the following steps: the surface of Nb to be welded is polished with 240# SiC sandpaper, 500# SiC sandpaper and 1000# SiC sandpaper in sequence, then ultrasonically cleaned in anhydrous ethanol, and finally dried. The rest is the same as specific embodiments 1 to 5.

[0033] Specific embodiment 7: This embodiment is different from specific embodiments 1 to 6 in that the TiNiNb foil described in step 2 is a pretreated TiNiNb foil, and the pretreatment is specifically performed according to the following steps: the upper and lower surfaces of the TiNiNb foil are polished with 60#SiC sandpaper, 240#SiC sandpaper, 1000#SiC sandpaper and 2000#SiC sandpaper in sequence until they are bright, then ultrasonically cleaned in anhydrous ethanol, and finally dried. The rest is the same as specific embodiments 1 to 6.

[0034] Specific embodiment 8: This embodiment differs from Specific embodiments 1 to 7 in that: a cellulose / ethanol binder is coated between every two layers of the assembled component described in step 2; the mass ratio of cellulose to ethanol in the cellulose / ethanol binder is 1g:(5-10)mL; the cellulose is cellulose acetate, carboxymethyl cellulose or microcrystalline cellulose. The rest is the same as Specific embodiments 1 to 7.

[0035] Specific embodiment 9: This embodiment differs from any one of the specific embodiments 1 to 8 in that: in step 3, the vacuum degree is 10 -4 ~10 -5Pa and the temperature is 1100° C. to 1250° C., and the temperature is kept for 5 to 15 minutes. The rest is the same as the specific embodiments 1 to 8.

[0036] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that: in step 3, the temperature is first raised to 100°C to 150°C within 8min to 20min, then raised to 950°C to 1050°C within 80min to 100min, and finally raised to 1100°C to 1250°C within 40min to 60min; in step 3, the temperature is first lowered to 900°C to 1050°C within 90min to 150min, then lowered to 150°C to 250°C within 150min to 200min, and finally lowered to below 100°C with the furnace. The rest is the same as specific embodiments 1 to 9.

[0037] The following examples are used to verify the beneficial effects of the present invention:

[0038] Embodiment 1:

[0039] A network intermediate layer auxiliary brazing C f The preparation method of the / SiC / Nb corrosion resistant joint is carried out according to the following steps:

[0040] 1. Under room temperature and normal pressure, the nickel foam was immersed in 15.6% by mass dilute hydrochloric acid for 10 minutes, then immersed in deionized water for 30 minutes, rinsed with deionized water, and then ultrasonically cleaned in anhydrous ethanol for 15 minutes, and finally dried with cold air from a hair dryer to obtain the acid-treated nickel foam;

[0041] 2. C f / SiC ceramic matrix composites, Nb, TiNiNb foils and acid-treated nickel foams were prepared according to the parent material C f / SiC / TiNiNb / foam nickel / TiNiNb / parent material Nb structure is assembled to obtain an assembled component;

[0042] 3. Place the assembled components in a vacuum brazing furnace and maintain the vacuum degree at 10 -5 Pa, firstly heat up to 100℃ in 7min, then heat up to 1000℃ in 90min, and finally heat up to 1200℃ in 50min. Keep the temperature at 1200℃ for 10min, then cool down to 1000℃ in 100min, then cool down to 200℃ in 160min, and finally cool down to below 100℃ with the furnace. Take out the weldment and get the network intermediate layer auxiliary brazing C f / SiC / Nb corrosion resistant joint.

[0043] The average pore diameter of the nickel foam described in step 1 is 150 μm, the porosity is 50%, and the size is 5 mm×5 mm×2 mm (thickness).

[0044] The TiNiNb foil described in step 2 is Ti 45 Ni 45 Nb 10 , dimensions are 5mm×5mm×0.3mm (thickness).

[0045] C described in step 2 f The SiC ceramic matrix composite material is prepared by three-dimensional woven carbon fiber chemical vapor deposition, with a porosity of 10% to 15%, a volume percentage of carbon fiber of 45% to 50%, a size of 5mm×5mm×5mm, and a pretreated C f / SiC ceramic matrix composite material, the pretreatment is specifically carried out in the following steps: f The surface to be welded of the SiC / SiC ceramic-based composite material (the surface where the fiber bundle area per unit area accounts for more than 60% is the surface to be welded) was polished with 300# gold sandpaper, 600# metallographic sandpaper and 1000# metallographic sandpaper in turn, then ultrasonically cleaned in anhydrous ethanol for 15 minutes, and finally dried at 80°C for 2 hours.

[0046] The size of Nb described in step 2 is 10mm×10mm×5mm, and it is pretreated Nb. The pretreatment is specifically carried out according to the following steps: the surface to be welded (10mm×10mm) of Nb is polished with 240#SiC sandpaper, 500#SiC sandpaper and 1000#SiC sandpaper in turn, and then ultrasonically cleaned in anhydrous ethanol for 15 minutes, and finally dried at a temperature of 80°C for 2 hours.

[0047] The TiNiNb foil described in step 2 is a pretreated TiNiNb foil, and the pretreatment is specifically carried out according to the following steps: the upper and lower surfaces of the TiNiNb foil are polished to brightness with 60#SiC sandpaper, 240#SiC sandpaper, 1000#SiC sandpaper and 2000#SiC sandpaper in sequence, and then ultrasonically cleaned in anhydrous ethanol for 15 minutes, and finally dried at a temperature of 80°C for 2 hours.

[0048] A cellulose / ethanol adhesive is coated between every two layers of the assembled components described in step 2, with a coating thickness of 1 mm. After bonding, the components are naturally placed until the adhesive solidifies. The mass ratio of cellulose to the volume of ethanol in the cellulose / ethanol adhesive is 1 g:6 mL. The cellulose is cellulose acetate CA.

[0049] Comparative experiment: The difference between this comparative experiment and Example 1 is that in step 2, C f / SiC ceramic matrix composites, Nb and TiNiNb foils are based on the base material C f / SiC / TiNiNb / parent material Nb structure is assembled to obtain an assembled component; step three obtains C without intermediate layer brazing f / SiC / Nb joint. Others are the same as those in the first embodiment.

[0050] Figure 1 The network intermediate layer auxiliary brazing C prepared in Example 1 f / SiC / Nb corrosion-resistant joint microstructure, A is TiNi phase, B is Nb(s,s) phase; it can be seen from the figure that after the introduction of nickel foam as a network intermediate layer into the joint, the phases of the joint are evenly distributed without obvious agglomeration, the interface crack size is small, and the TiNi phase and Nb(s,s) phase with good corrosion resistance are distributed in large quantities and evenly in the weld.

[0051] The shear performance test was carried out under room temperature and pressure conditions, with the pressure head speed being 0.5 mm / min. The network intermediate layer prepared in Example 1 assisted brazing C f The room temperature shear strength of / SiC / Nb anti-corrosion joint is 125.78MPa.

[0052] Figure 2 C brazed without intermediate layer prepared for comparative experiment f Microstructure of the / SiC / Nb joint, A is the brittle phase Ti (Nb, Ni); as can be seen from the figure, the joint structure is mainly layered in the absence of an intermediate layer, the gray-white brittle phase Ti (Nb, Ni) is continuously distributed at the interface of the parent material, the amount of corrosion-resistant phase and strengthening phase generated is small, and C f Large-sized crack defects appear at the / SiC interface.

[0053] The shear performance test was carried out under room temperature and normal pressure conditions, with a pressure head speed of 0.5 mm / min. The C brazed without intermediate layer prepared in the experiment was compared. f The room temperature shear strength of the / SiC / Nb joint is 33.78MPa.

[0054] Figure 3 The network intermediate layer auxiliary brazing C prepared in Example 1 f / SiC / Nb corrosion resistant joints and comparative experiments on C brazed joints without intermediate layer f / SiC / Nb joints were subjected to accelerated corrosion tests after immersion in 15wt.% NaCl solution at room temperature for 28 days. (a) is a comparative experiment, and (b) is Example 1. It can be seen from the figure that large-sized hole defects appear in the joint without intermediate layer reinforcement, and due to the good reinforcement effect of nickel foam, the corrosion area of ​​the reinforced joint is much lower than that of the joint without intermediate layer and there is no obvious hole defect.

[0055] The shear performance test was carried out at room temperature and pressure, with a pressure head speed of 0.5 mm / min; Figure 4 The network intermediate layer auxiliary brazing C prepared in Example 1 f / SiC / Nb corrosion resistant joints and comparative experiments on C brazed joints without intermediate layer f Figure 1 is a time-varying curve of the shear strength of the / SiC / Nb joint after an immersion accelerated corrosion test in a 15wt.% NaCl solution at room temperature for 28 days, (a) is a comparative experiment, and (b) is Example 1. It can be seen from the figure that after the corrosion is completed, the strength retention rate of the joint without intermediate layer reinforcement is only 46.7%, while the shear strength retention rate of the joint brazed with foam nickel intermediate layer is as high as 73.8%.

Claims

1. A network intermediate layer auxiliary brazing C f / SiC / Nb corrosion resistant joint preparation method, characterized in that It is carried out in the following steps:

1. Immersing the nickel foam in dilute hydrochloric acid, then washing and drying, to obtain the acid-treated nickel foam; 2. C f / SiC ceramic matrix composites, Nb, TiNiNb foils and acid-treated nickel foams were prepared according to the parent material C f / SiC / TiNiNb / foam nickel / TiNiNb / parent material Nb structure is assembled to obtain an assembled component; 3. Place the assembled components in a vacuum brazing furnace, keep them warm for 5-15 minutes under vacuum environment and temperature of 1100-1250°C, then cool them down to below 100°C and take out the welded parts to obtain the network intermediate layer auxiliary brazing C f / SiC / Nb corrosion resistant joint.

2. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that The nickel foam described in step 1 has a pore diameter of 100 μm to 200 μm, a porosity of 30% to 70%, and a thickness of 1 mm to 4 mm.

3. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that In step 1, the nickel foam is immersed in 3.5% to 25% by mass dilute hydrochloric acid at room temperature and pressure for 5 minutes to 15 minutes.

4. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that The atomic content ratio of Ti to Ni in the TiNiNb foil described in step 2 is 1:1, and the atomic percentage content of Nb is 5% to 15%; the thickness of the TiNiNb foil described in step 2 is 0.1mm to 0.5mm.

5. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that C described in step 2 f The C / SiC ceramic matrix composite material is pretreated f / SiC ceramic matrix composite material, and the pretreatment is specifically carried out in the following steps: C f The surface to be welded of the SiC / SiC ceramic matrix composite material was polished with 300# gold sandpaper, 600# metallographic sandpaper and 1000# metallographic sandpaper in turn, then ultrasonically cleaned in anhydrous ethanol, and finally dried.

6. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that The Nb described in step 2 is pretreated Nb, and the pretreatment is specifically performed according to the following steps: the surface of Nb to be welded is polished with 240# SiC sandpaper, 500# SiC sandpaper and 1000# SiC sandpaper in sequence, then ultrasonically cleaned in anhydrous ethanol, and finally dried.

7. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that The TiNiNb foil described in step 2 is a pretreated TiNiNb foil, and the pretreatment is specifically carried out according to the following steps: the upper and lower surfaces of the TiNiNb foil are polished to a bright finish with 60#SiC sandpaper, 240#SiC sandpaper, 1000#SiC sandpaper and 2000#SiC sandpaper in sequence, then ultrasonically cleaned in anhydrous ethanol, and finally dried.

8. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that A cellulose / ethanol binder is coated between every two layers of the assembled component described in step 2; the mass ratio of cellulose to ethanol in the cellulose / ethanol binder is 1g:(5-10)mL; and the cellulose is cellulose acetate, carboxymethyl cellulose or microcrystalline cellulose.

9. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that In step 3, the vacuum degree is 10 -4 ~10 -5 Under the conditions of Pa and temperature of 1100℃~1250℃, keep warm for 5min~15min.

10. A network intermediate layer auxiliary brazing C according to claim 1 f / SiC / Nb corrosion resistant joint preparation method, characterized in that In step three, the temperature is first raised to 100°C to 150°C within 8min to 20min, then raised to 950°C to 1050°C within 80min to 100min, and finally raised to 1100°C to 1250°C within 40min to 60min; in step three, the temperature is first lowered to 900°C to 1050°C within 90min to 150min, then lowered to 150°C to 250°C within 150min to 200min, and finally lowered to below 100°C with the furnace.

Citation Information

Patent Citations

  • Brazing material and preparation method thereof as well as brazing method using the material

    CN101327551A

  • Method for relieving residual stress of brazed joint

    CN103143805A

  • Graphene auxiliary brazing method for ceramic matrix composite material and metal material

    CN103341674A

  • High-temperature solder of brazing ceramic, ceramic matrix composite and metal as well as preparation method and using method of high-temperature solder

    CN104551442A

  • METHOD OF JOINING PARTS MADE OF SiC-BASED MATERIALS BY NON-REACTIVE BRAZING WITH ADDITION OF A REINFORCEMENT. BRAZING COMPOSITIONS AND JOINT AND ASSEMBLY THAT ARE OBTAINED BY SUCH A METHOD

    US20130064602A1