Welding method of fillet weld

By pre-mixing nano-titanium diboride powder and copper powder zinc powder, combining drawing coating and layer-by-layer self-assembly processes, multi-coated welding wire is formed, and the wear resistance of welding wire in the existing aluminum alloy corner weld welding technology and The problem of insufficient mechanical properties has significantly improved the welding quality and the service life of the welding wire.

CN119057306APending Publication Date: 2024-12-03CHANGZHOU HAIBAO WELDING & CUTTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411228123.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the existing aluminum alloy corner weld welding technology, the selection and process optimization of welding wires are insufficient, resulting in poor deformation, cracks and wear resistance in the welding area, affecting welding quality and product performance.

Method used

Using a welding method of fillet welds, welding wire is prepared by pre-mixing nano-titanium diboride powder, copper powder and zinc powder to metal components, and drawing and coating on the surface of the welding wire and self-assembly layer by layer. The process is to form multi-coated welding wire, combining silicon carbide whiskers, reducing graphene oxide and polyvinyl alcohol to improve the wear resistance and mechanical properties of the welding wire.

Benefits of technology

It significantly improves welding stability, wear resistance and mechanical properties, extends the service life of welding wire, and ensures high quality and reliability of welding materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005025268580000071
    Figure BDA0005025268580000071
  • Figure BDA0005025268580000081
    Figure BDA0005025268580000081
Patent Text Reader

Abstract

The invention relates to the technical field of welding, in particular to a fillet weld welding method. The welding wire is prepared by adding the pure aluminum block, the core-shell titanium diboride powder and the pure magnesium block. Adding calcium carbonate, sodium fluoride, silicon dioxide, Ni-Fe, molybdenum disulfide and titanium dioxide to obtain active slurry; the wear-resistant slurry is obtained by adding silicon carbide whiskers, reduced graphene oxide, polyvinyl alcohol and deionized water. And the surface of the welding wire is subjected to a drawing and coating process, active slurry is coated, and the single-coating welding wire is prepared. And the single-coating welding wire is spin-coated with wear-resistant slurry through a layer-by-layer self-assembly process, and the multi-coating welding wire is prepared. And the multi-coating welding wire and the aluminum alloy plate are subjected to surface treatment through acetone, then the multi-coating welding wire is used for welding the aluminum alloy plate, and the welding material is obtained. The welding material prepared through the method has good mechanical performance and welding performance, and therefore the welding material has wide application prospects in the technical field of welding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, in particular to a welding method for a fillet weld. Background Art

[0002] The welding of aluminum alloy fillet welds has important technical and economic value in modern industry. Aluminum alloys are widely used in aerospace, automobile manufacturing, construction engineering and other fields due to their excellent lightweight, corrosion resistance and thermal conductivity. As a common connection method in aluminum alloy structures, the welding quality of fillet welds directly affects the performance and safety of the products, as follows: First, the development of modern aluminum alloy fillet weld welding technology enables aluminum alloy structures to achieve higher strength and sealing. Through advanced welding processes and material selection, the deformation and cracks in the welding area can be effectively reduced, the strength and durability of the weld can be improved, and the reliability and service life of the overall structure can be enhanced. In addition, modern welding technology also enables aluminum alloy fillet welds to perform well in a variety of application environments. Through appropriate welding method selection and process optimization, the metal structure and chemical properties of the welding area can be effectively controlled. Among them, welding wire plays a vital role in the welding process of fillet welds, and its welding performance, surface wear resistance and mechanical strength directly affect the welding quality and the performance of the final product.

[0003] In modern industry, the selection of welding wire should be able to match well with the base material to be welded to ensure the stability and fluidity of the molten pool during welding. Good welding performance means that the welding wire can melt quickly and fully fuse with the base material to form a solid weld, thereby ensuring welding strength and sealing. In addition, the surface wear resistance of the welding wire directly affects the operational stability and the finish of the weld during welding. The high wear resistance of the welding wire surface means that it is not easy to generate debris or contaminate the molten pool during welding, which helps to maintain the cleanliness and uniformity of the weld. Finally, the mechanical strength of the welding wire directly affects the mechanical properties of the welded joint. High-strength welding wire can provide better welded joint strength and tensile properties, thereby enhancing the durability and load capacity of the overall structure.

[0004] In order to overcome the defects of the prior art, the present invention provides a welding method for a fillet weld. Summary of the invention

[0005] The object of the present invention is to provide a welding method for a fillet weld to solve the problems in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] A method for preparing a fillet weld wire comprises the following steps:

[0008] Step 1: Melt the pure aluminum block at 800-900°C to obtain a melt, then add the core-shell titanium diboride powder to the melt, stir it thoroughly for 40-60 minutes, then cool it to 650-700°C and add the pure magnesium block, let it stand for 5-10 minutes, then add the reaction liquid to the mold at 700-720°C to obtain an ingot, and then homogenize it to obtain a welding wire;

[0009] Step 2: preparing a single-coated welding wire by performing a drawing and coating process on the surface of the welding wire;

[0010] Step three: dispersing silicon carbide whiskers and reduced graphene oxide in deionized water to obtain a dispersion; dissolving polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol solution; adding the dispersion to the polyvinyl alcohol solution, stirring thoroughly for 30-40 minutes to obtain a wear-resistant slurry; spin-coating the wear-resistant slurry onto the surface of a single-coated welding wire through a layer-by-layer self-assembly process to obtain a multi-coated welding wire.

[0011] More optimally, in step 1, nano titanium diboride powder, copper powder and zinc powder are mixed and ball milled for 9-12 hours at a rotation speed of 120-140 rpm / min and a revolution speed of 1-2 rpm / min to obtain core-shell titanium diboride powder; wherein the ball-to-material ratio is 5:(1-2).

[0012] More optimally, by weight, 17-20 parts of nano titanium diboride powder, 25-30 parts of copper powder, and 95-100 parts of zinc powder.

[0013] More optimally, in step one, the contents of the components of the welding wire are: by mass, 1200-1300 parts of pure aluminum block, 130-150 parts of core-shell titanium diboride powder, and 25-30 parts of pure magnesium block.

[0014] More optimally, in step 2, the drawing coating process is specifically as follows: the active slurry is coated on the surface of the welding wire through the mechanical extrusion action of the wire drawing die to obtain a single-coated welding wire with a coating thickness of 50-70 μm.

[0015] More optimally, the contents of the components of the active slurry are: by mass fraction, 8-10% calcium carbonate, 7-9% sodium fluoride, 25-35% silicon dioxide, 20-30% Ni-Fe, 7-9% molybdenum disulfide, and the balance is titanium dioxide.

[0016] More optimally, in step three, the reaction mass ratio of silicon carbide whiskers, native graphene oxide and polyvinyl alcohol is (0.7-0.9):0.3:1.

[0017] More optimally, in step three, the layer-by-layer self-assembly process is as follows: spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire, rotate at 600-700rpm for 10s and 2000-2500rpm for 15s to obtain the first layer, repeat the above steps to deposit 20-25 layers, and then dry at 100-120℃ for 2-4h to obtain a multi-coated welding wire.

[0018] A fillet weld welding method comprises the following specific steps: surface treating a multi-coated welding wire and an aluminum alloy plate with acetone, welding the aluminum alloy plate with the multi-coated welding wire, butting the plate and opening a 60-70° groove to obtain a welding material.

[0019] More optimally, the welding current is 150-200A, the welding speed is 40-45mm / min, and the argon gas flow rate is 20-30L / min.

[0020] Beneficial effects of the present invention:

[0021] The present invention prepares welding wire by adding pure aluminum block, core-shell titanium diboride powder and pure magnesium block raw materials. Active slurry is obtained by adding calcium carbonate, sodium fluoride, silicon dioxide, Ni-Fe, molybdenum disulfide and titanium dioxide; wear-resistant slurry is obtained by adding silicon carbide whiskers, reduced graphene oxide, polyvinyl alcohol and deionized water. The surface of the welding wire is subjected to a drawing and coating process, and the active slurry is coated to prepare a single-coated welding wire. The single-coated welding wire is subjected to a layer-by-layer self-assembly process, and the wear-resistant slurry is spin-coated to prepare a multi-coated welding wire. The multi-coated welding wire and the aluminum alloy plate are surface-treated with acetone, and the aluminum alloy plate is welded with the multi-coated welding wire to obtain a welding material.

[0022] The present invention is characterized in that, in step one, nano titanium diboride powder, copper powder and zinc powder are first pre-mixed to obtain a core-shell titanium diboride powder, and then the core-shell titanium diboride powder is added to the metal component to prepare the welding wire. The beneficial effects of this step are: on the one hand, by pre-ball milling, the particle size of the core-shell titanium diboride powder is more uniform, and the surface is smoother, which is conducive to the uniform dispersion and mixing of subsequent reactions. This uniformity can ensure the uniform distribution of particles after being added to the melt, thereby effectively improving the process stability of the welding wire and the consistency of product quality. On the other hand, the specific surface area and the number of active sites of the powder can be increased by pre-ball milling, so that the core-shell titanium diboride powder is easier to react with metal elements such as aluminum and magnesium in the melt. High reactivity helps to promote the formation of intermetallic compounds at a lower temperature, thereby improving the comprehensive properties of the welding wire, such as hardness, wear resistance and corrosion resistance.

[0023] The feature of the present invention is that in step 2, the surface of the welding wire is subjected to a drawing and coating process, and an active slurry is coated to prepare a single-coated welding wire. In this step, by adding oxides such as silicon dioxide and titanium dioxide to the coating components, the surface tension of the molten droplet can be significantly reduced during welding, and the molten droplet can be promoted to be refined, thereby improving the welding stability. In addition, by first coating a layer of coating on the welding wire, it can be used as a base coating to improve the adhesion stability of the next coating and ensure the stability and durability of the second layer of coating on the surface of the welding wire. In step 3, a wear-resistant slurry is obtained by adding silicon carbide whiskers, reduced graphene oxide, polyvinyl alcohol, and deionized water; the single-coated welding wire is subjected to a layer-by-layer self-assembly process, and the wear-resistant slurry is spin-coated to prepare a multi-coated welding wire. In this step, silicon carbide whiskers, reduced graphene oxide, and polyvinyl alcohol are mixed, and polyvinyl alcohol molecules can be used to form an adsorption layer on the surface of silicon carbide whiskers, and interact with reduced graphene oxide in the coating to form hydrogen bonds, thereby enhancing the adhesion between silicon carbide whiskers and the coating substrate, preventing whiskers from peeling off during use, and improving the stability and durability of the coating; in addition, polyvinyl alcohol molecules can also improve the adhesion between reduced graphene oxide sheets, avoid peeling off, and form a compact coating structure. Therefore, due to the high molecular weight and polyhydroxy structure of polyvinyl alcohol molecules, their addition to reduced graphene oxide and silicon carbide whisker dispersions can significantly improve the adhesion and stability of wear-resistant slurry. This not only improves the mechanical properties of the coating, but also can reduce wear and fatigue during use, significantly improve the wear resistance of the welding wire, and extend the service life of the multi-layer welding wire. Therefore, by using multi-coated welding wire to weld aluminum alloy plates, the obtained welding material has good mechanical properties, wear resistance and welding stability. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Source of raw materials:

[0026] Nano titanium diboride powder, provided by Qinghe Chaotai Metal Materials Co., Ltd., with a particle size of 2000 mesh; copper powder, provided by Hebei Yinbai Alloy Welding Material Co., Ltd., with a particle size of 500nm; zinc powder, provided by Jinzhou Wanda Zinc Co., Ltd., with a particle size of 300 mesh; silicon carbide whiskers, provided by Qinghe Chaotai Metal Materials Co., Ltd., with a particle size of 2000 mesh; reduced graphene oxide, provided by Dongguan Kelude New Energy Technology Co., Ltd., model TG1600; polyvinyl alcohol, provided by Chaohu Desheng Chemical Construction Co., Ltd., model 2488; Ni-Fe, with a particle size of 500 mesh and a metal Ni content of 45wt%; aluminum alloy plate is 7055 aluminum alloy plate, with a size of 300mm×150mm×5mm; in terms of mass, 1 portion is 1g.

[0027] Example 1: Step 1: S1: 17 g of nano titanium diboride powder, 25 g of copper powder, and 95 g of zinc powder were mixed, and ball-milled for 12 h at a rotation speed of 120 rpm / min and a revolution speed of 1 rpm / min to obtain core-shell titanium diboride powder; wherein the ball-to-material ratio was 5:1.5;

[0028] S2: 1200g of pure aluminum block is melted at 900°C to obtain a melt, and then 130g of core-shell titanium diboride powder is added to the melt, fully stirred for 60min, and then cooled to 700°C and 25g of pure magnesium block is added. The mixture is allowed to stand for 10min, and then the reaction solution is added to a mold at 720°C to obtain an ingot, which is then homogenized to obtain a welding wire;

[0029] Step 2: A single-coated welding wire is prepared by a drawing and coating process on the surface of the welding wire; the drawing and coating process is specifically as follows: the active slurry is coated on the surface of the welding wire through the mechanical extrusion of the wire drawing die to obtain a single-coated welding wire with a coating thickness of 60 μm; wherein, by mass fraction, 8% calcium carbonate, 7% sodium fluoride, 25% silicon dioxide, 20% Ni-Fe, 9% molybdenum disulfide, and 31% titanium dioxide;

[0030] Step 3: Disperse 8g of silicon carbide whiskers and 3g of reduced graphene oxide in deionized water to obtain a dispersion; dissolve 10g of polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol solution; add the dispersion to the polyvinyl alcohol solution, stir thoroughly for 40 minutes, and obtain a wear-resistant slurry; spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire through a layer-by-layer self-assembly process to obtain a multi-coated welding wire; the layer-by-layer self-assembly process is specifically as follows: spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire, rotate at 700rpm for 10s and 2500rpm for 15s to obtain the first layer, repeat the above steps to deposit 25 layers, and then dry at 120°C for 4h to obtain a multi-coated welding wire;

[0031] Step 4: Use acetone to surface treat the multi-coated welding wire and the aluminum alloy plate, then use the multi-coated welding wire to weld the aluminum alloy plate, adopt a butt joint method and open a 70° groove to obtain welding materials; the welding current is 200A, the welding speed is 45mm / min, and the argon gas flow rate is 30L / min.

[0032] Example 2: Step 1: S1: 17 g of nano titanium diboride powder, 25 g of copper powder, and 95 g of zinc powder were mixed, and ball-milled for 10 h at a rotation speed of 120 rpm / min and a revolution speed of 1 rpm / min to obtain core-shell titanium diboride powder; wherein the ball-to-material ratio was 5:1.5;

[0033] S2: 1200g of pure aluminum block was melted at 850°C to obtain a melt, and then 130g of core-shell titanium diboride powder was added to the melt, and the mixture was stirred for 50min. After the mixture was cooled to 670°C, 25g of pure magnesium block was added, and the mixture was allowed to stand for 8min. The reaction solution was then added to a mold at 710°C to obtain an ingot, and then subjected to a homogenization treatment to obtain a welding wire.

[0034] Step 2: A single-coated welding wire is prepared by a drawing and coating process on the surface of the welding wire; the drawing and coating process is specifically as follows: the active slurry is coated on the surface of the welding wire through the mechanical extrusion of the wire drawing die to obtain a single-coated welding wire with a coating thickness of 60 μm; wherein, by mass fraction, 8% calcium carbonate, 7% sodium fluoride, 25% silicon dioxide, 20% Ni-Fe, 9% molybdenum disulfide, and 31% titanium dioxide;

[0035] Step 3: Disperse 8g of silicon carbide whiskers and 3g of reduced graphene oxide in deionized water to obtain a dispersion; dissolve 10g of polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol solution; add the dispersion to the polyvinyl alcohol solution, stir thoroughly for 35 minutes, and obtain a wear-resistant slurry; spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire through a layer-by-layer self-assembly process to obtain a multi-coated welding wire; the layer-by-layer self-assembly process is specifically as follows: spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire, rotate at 650rpm for 10s and 2250rpm for 15s to obtain the first layer, repeat the above steps to deposit 25 layers, and then dry at 110°C for 3h to obtain a multi-coated welding wire;

[0036] Step 4: Use acetone to surface treat the multi-coated welding wire and the aluminum alloy plate, then use the multi-coated welding wire to weld the aluminum alloy plate, adopt a butt-jointing method and open a 65° groove to obtain welding materials; the welding current is 170A, the welding speed is 43mm / min, and the argon gas flow rate is 25L / min.

[0037] Example 3: Step 1: S1: 17 g of nano titanium diboride powder, 25 g of copper powder, and 95 g of zinc powder were mixed, and ball-milled for 9 h at a rotation speed of 120 rpm / min and a revolution speed of 1 rpm / min to obtain core-shell titanium diboride powder; wherein the ball-to-material ratio was 5:1.5;

[0038] S2: 1200g of pure aluminum block was melted at 800°C to obtain a melt, and then 130g of core-shell titanium diboride powder was added to the melt, and the mixture was fully stirred for 40min. After the temperature was lowered to 650°C, 25g of pure magnesium block was added, and the mixture was allowed to stand for 5min. The reaction solution was then added to a mold at 700°C to obtain an ingot, and then subjected to a homogenization treatment to obtain a welding wire.

[0039] Step 2: A single-coated welding wire is prepared by a drawing and coating process on the surface of the welding wire; the drawing and coating process is specifically as follows: the active slurry is coated on the surface of the welding wire through the mechanical extrusion of the wire drawing die to obtain a single-coated welding wire with a coating thickness of 60 μm; wherein, by mass fraction, 8% calcium carbonate, 7% sodium fluoride, 25% silicon dioxide, 20% Ni-Fe, 9% molybdenum disulfide, and 31% titanium dioxide;

[0040] Step 3: Disperse 8g of silicon carbide whiskers and 3g of reduced graphene oxide in deionized water to obtain a dispersion; dissolve 10g of polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol solution; add the dispersion to the polyvinyl alcohol solution, stir thoroughly for 30 minutes, and obtain a wear-resistant slurry; spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire through a layer-by-layer self-assembly process to obtain a multi-coated welding wire; the layer-by-layer self-assembly process is specifically as follows: spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire, rotate at 600rpm for 10s and 2000rpm for 15s to obtain the first layer, repeat the above steps to deposit 25 layers, and then dry at 100°C for 2h to obtain a multi-coated welding wire;

[0041] Step 4: Use acetone to surface treat the multi-coated welding wire and the aluminum alloy plate, then use the multi-coated welding wire to weld the aluminum alloy plate, adopt a butt-jointing method and open a 60° groove to obtain welding materials; the welding current is 150A, the welding speed is 40mm / min, and the argon gas flow rate is 20L / min.

[0042] Comparative Example 1: The preparation of single-coated welding wire in step 2 and the preparation of multi-coated welding wire in step 3 are removed, and the rest is the same as in Example 1, and the specific steps are as follows: Step 1: S1: 17g of nano titanium diboride powder, 25g of copper powder, and 95g of zinc powder are mixed, and ball milled for 12h at a rotation speed of 120rpm / min and a revolution speed of 1rpm / min to obtain core-shell titanium diboride powder; wherein the ball-to-material ratio is 5:1.5;

[0043] S2: 1200g of pure aluminum block is melted at 900°C to obtain a melt, and then 130g of core-shell titanium diboride powder is added to the melt, fully stirred for 60min, and then cooled to 700°C and 25g of pure magnesium block is added. The mixture is allowed to stand for 10min, and then the reaction solution is added to a mold at 720°C to obtain an ingot, which is then homogenized to obtain a welding wire;

[0044] Step 2: Use acetone to surface treat the welding wire and the aluminum alloy plate, then use the welding wire to weld the aluminum alloy plate, adopt a butt joint method and open a 70° groove to obtain welding materials; the welding current is 200A, the welding speed is 45mm / min, and the argon gas flow rate is 30L / min.

[0045] Comparative Example 2: The original nano titanium diboride powder, copper powder and zinc powder in step 1 S1 are directly added to the melt of S2 to prepare a welding wire. The rest is the same as Example 1, and the specific steps are as follows: Step 1: Melt 1200g of pure aluminum block at 900°C to obtain a melt, then add 17g of nano titanium diboride powder, 25g of copper powder and 95g of zinc powder to the melt, stir well for 60min, cool to 700°C, add 25g of pure magnesium block, let stand for 10min, and then add the reaction solution to a mold at 720°C to obtain an ingot, which is then homogenized to obtain a welding wire;

[0046] Step 2: A single-coated welding wire is prepared by a drawing and coating process on the surface of the welding wire; the drawing and coating process is specifically as follows: the active slurry is coated on the surface of the welding wire through the mechanical extrusion of the wire drawing die to obtain a single-coated welding wire with a coating thickness of 60 μm; wherein, by mass fraction, 8% calcium carbonate, 7% sodium fluoride, 25% silicon dioxide, 20% Ni-Fe, 9% molybdenum disulfide, and 31% titanium dioxide;

[0047] Step 3: Disperse 8g of silicon carbide whiskers and 3g of reduced graphene oxide in deionized water to obtain a dispersion; dissolve 10g of polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol solution; add the dispersion to the polyvinyl alcohol solution, stir thoroughly for 40 minutes, and obtain a wear-resistant slurry; spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire through a layer-by-layer self-assembly process to obtain a multi-coated welding wire; the layer-by-layer self-assembly process is specifically as follows: spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire, rotate at 700rpm for 10s and 2500rpm for 15s to obtain the first layer, repeat the above steps to deposit 25 layers, and then dry at 120°C for 4h to obtain a multi-coated welding wire;

[0048] Step 4: Use acetone to surface treat the multi-coated welding wire and the aluminum alloy plate, then use the multi-coated welding wire to weld the aluminum alloy plate, adopt a butt joint method and open a 70° groove to obtain welding materials; the welding current is 200A, the welding speed is 45mm / min, and the argon gas flow rate is 30L / min.

[0049] Detection test:

[0050] Mechanical properties test: The present invention uses a multi-coated welding wire to weld aluminum alloy plates to obtain welding materials, and uses a wire cutting machine to cut the welded joint to obtain a 10mm×10mm×10mm sample. The hardness of a material is the most direct way to characterize mechanical properties. This test uses Vickers hardness to characterize the hardness of the sample. The sample surface is first polished with sandpaper, and then five points are selected on the surface of each sample for measurement, and the average value is taken as the average hardness.

[0051] Wear resistance test: The present invention uses multi-coated welding wire to weld aluminum alloy plates to obtain welding materials, and uses a wire cutting machine to cut the welded joint to obtain a sample with a diameter of 4 mm and a length of 15 mm. The MMG-5G friction and wear high temperature end surface tester is used to test the loss mass of the sample before and after wear at room temperature, with a load of 200N. The results are as follows:

[0052]

[0053]

[0054] Conclusion: The dosage of Examples 1 to 3 remains unchanged, and only some reaction parameters are modified. From the experimental data, it can be seen that there is no obvious fluctuation in the performance of the samples.

[0055] Comparative Example 1: The single-coated welding wire preparation in step 2 and the multi-coated welding wire preparation in step 3 are removed, and the rest is the same as Example 1. It can be seen from the experimental data that compared with Example 1, the hardness is reduced to 170HV, and the wear amount is increased to 35mg. The reasons are analyzed as follows: in the multi-coated welding wire prepared by the present invention, the base coating contains components such as silicon dioxide and titanium dioxide, which can effectively improve the welding performance; the second coating contains components such as silicon carbide whiskers, reduced graphene oxide, and polyvinyl alcohol, which can effectively improve the wear resistance and mechanical properties of the welding wire surface. Therefore, after removing steps 2 and 3, the hardness is reduced, the wear amount is increased, and the mechanical properties and wear resistance are reduced.

[0056] Comparative Example 2: The original nano titanium diboride powder, copper powder and zinc powder in step 1 S1 are directly added to the melt of S2 to prepare a welding wire. The rest is the same as Example 1, and the hardness is reduced to 148HV. The reason is analyzed as follows: In the embodiment, the nano titanium diboride powder, copper powder and zinc powder are pre-mixed and ball-milled to obtain a core-shell titanium diboride powder, and then the core-shell titanium diboride powder is added to the metal component. The prepared welding wire has good partial dispersion performance and comprehensive mechanical properties. Therefore, after replacing this step with the direct addition of the three components, the hardness is significantly reduced compared with the original embodiment, and the mechanical properties are significantly reduced.

[0057] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0058] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a welding wire for a fillet weld, characterized in that: The following steps are involved: Step 1: Melt the pure aluminum block at 800-900°C to obtain a melt, then add the core-shell titanium diboride powder to the melt, stir it thoroughly for 40-60 minutes, then cool it to 650-700°C and add the pure magnesium block, let it stand for 5-10 minutes, then add the reaction liquid to the mold at 700-720°C to obtain an ingot, and then homogenize it to obtain a welding wire; Step 2: preparing a single-coated welding wire by performing a drawing and coating process on the surface of the welding wire; Step three: dispersing silicon carbide whiskers and reduced graphene oxide in deionized water to obtain a dispersion; dissolving polyvinyl alcohol in deionized water to obtain a polyvinyl alcohol solution; adding the dispersion to the polyvinyl alcohol solution, stirring thoroughly for 30-40 minutes to obtain a wear-resistant slurry; spin-coating the wear-resistant slurry onto the surface of a single-coated welding wire through a layer-by-layer self-assembly process to obtain a multi-coated welding wire.

2. The method for preparing a fillet weld wire according to claim 1, characterized in that: In step 1, nano titanium diboride powder, copper powder and zinc powder are mixed, and ball milled for 9-12 hours at a rotation speed of 120-140 rpm / min and a revolution speed of 1-2 rpm / min to obtain core-shell titanium diboride powder; wherein the ball-to-material ratio is 5:(1-2).

3. The method for preparing a fillet weld wire according to claim 2, characterized in that: By mass, 17-20 parts of nano titanium diboride powder, 25-30 parts of copper powder, and 95-100 parts of zinc powder.

4. The method for preparing a fillet weld wire according to claim 1, characterized in that: In step 1, the contents of the components of the welding wire are: by mass, 1200-1300 parts of pure aluminum block, 130-150 parts of core-shell titanium diboride powder, and 25-30 parts of pure magnesium block.

5. The method for preparing a fillet weld wire according to claim 1, characterized in that: In step 2, the drawing coating process is specifically as follows: the active slurry is coated on the surface of the welding wire through the mechanical extrusion of the wire drawing die to obtain a single-coated welding wire with a coating thickness of 50-70 μm.

6. The method for preparing a fillet weld wire according to claim 5, characterized in that: The contents of the components of the active slurry are: by mass fraction, 8-10% calcium carbonate, 7-9% sodium fluoride, 25-35% silicon dioxide, 20-30% Ni-Fe, 7-9% molybdenum disulfide, and the balance is titanium dioxide.

7. The method for preparing a fillet weld wire according to claim 1, characterized in that: In step three, the reaction mass ratio of silicon carbide whiskers, native graphene oxide and polyvinyl alcohol is (0.7-0.9):0.3:

1.

8. The method for preparing a fillet weld wire according to claim 1, characterized in that: In step three, the layer-by-layer self-assembly process is specifically as follows: spin-coat the wear-resistant slurry onto the surface of the single-coated welding wire, rotate at 600-700rpm for 10s and 2000-2500rpm for 15s to obtain the first layer, repeat the above steps to deposit 20-25 layers, and then dry at 100-120℃ for 2-4h to obtain a multi-coated welding wire.

9. A method for welding a fillet weld, characterized in that: The specific steps are: using acetone to surface treat the multi-coated welding wire and the aluminum alloy plate, then using the multi-coated welding wire to weld the aluminum alloy plate, using a butt joint method and opening a 60-70° groove to obtain a welding material.

10. A fillet weld welding method according to claim 9, characterized in that: The welding current is 150-200A, the welding speed is 40-45mm / min, and the argon gas flow rate is 20-30L / min.