Preparation method and application of nickel-based amorphous alloy brazing material with high W content

By introducing B and Cr elements into nickel-based amorphous alloy brazing material, a high W content nickel-based amorphous alloy brazing material was designed, which solved the problem of difficulty in introducing high melting point W elements, and achieved low melting point and high mechanical Nickel-based amorphous alloy solder with performance, suitable for high-temperature alloy welding.

CN119057311APending Publication Date: 2024-12-03BEIHANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411392768.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-02-21
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In the prior art, it is difficult to introduce high melting point refractory metals such as W elements into nickel-based amorphous alloy brazing material, resulting in an increase in the alloy melting point and amorphous formation ability, which affects the mechanical properties of the welded joints.

Method used

By introducing the reduced melting elements B and Cr, a high W content of nickel-based amorphous alloy brazing components, such as Ni75W5B20 and Ni65Cr10W5B20, were designed, and amorphous alloy thin strips were prepared by vacuum high-frequency induction smelting and melt quenching method, and controlled Brazing temperature and time to avoid the formation of intermetallic compounds, forming a single W element solid solution structure.

Benefits of technology

It realizes a nickel-based amorphous alloy brazing material with high W content and low melting point, improves the room temperature and high temperature mechanical properties of the welded joints, and reaches the performance level of more than 80% of the base material, and is suitable for high-quality nickel-based high-temperature alloy brazing connections.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119057311A_ABST
    Figure CN119057311A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a high-W-content nickel-based amorphous alloy brazing material, and relates to the technical field of nickel-based high-temperature alloy welding. The component general formula of the brazing material is NiaWbBc, and a, b and c all represent atomic percent; b is equal to 5, c is equal to 20, a is equal to 100-b-c, and the melting point of the brazing material is 1095-1120 DEG C; the method specifically comprises the following steps: (1) converting atomic percent into mass percent according to the components of the brazing material, and accurately weighing Ni, W and B elementary substances as raw materials; (2) sequentially putting the raw materials into a vacuum high-frequency induction melting furnace, vacuumizing, filling argon as protective gas, and heating by a high-frequency power supply to obtain a master alloy ingot with uniform components; (3) after the master alloy ingot is crushed, an amorphous alloy brazing filler metal strip with the thickness being 30-70 microns and the width being larger than or equal to 10 mm is obtained through a melt rotary quenching rapid solidification method; in the step (2), the placing sequence of the raw materials is as follows: the elementary substance B is firstly and uniformly added, and finally the elementary substance Ni is added.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nickel-based high-temperature alloy welding, and in particular relates to a preparation method and application of a nickel-based amorphous alloy brazing material with a high W content. Background Art

[0002] As the "crown jewel of modern industry", the new generation of aircraft engines is developing towards high thrust-to-weight ratio and low fuel consumption rate, which requires the use temperature of hot end components such as combustion chambers to be higher and higher, and the loads on various components are also increasing. In order to meet the increasing working temperature, Ni-based high-temperature alloys are widely used in the manufacture of hot end components of engines. Due to the difficulty of overall casting of complex-shaped parts, and the need to cover the repair of turbine blades, welding work is essential in the use and repair of Ni-based high-temperature alloys.

[0003] Brazing is an important technical means in the process of connecting high-temperature alloys. Due to its low welding temperature, it has little impact on the parent material and can effectively avoid defects such as thermal cracks and pores in the process of connecting Ni-based high-temperature alloys. Brazing materials (brazine) are one of the important factors affecting the quality of brazing, and amorphous alloys are prepared through processes such as rapid solidification and mechanical alloying. They are a new type of alloy that combines the physical properties of metal, glass, liquid phase and solid phase. Thanks to the unique atomic arrangement structure and uniformity of chemical composition of amorphous alloys, common defects such as dislocations and grain boundaries in crystalline materials no longer exist in amorphous alloys, thus giving amorphous alloys the characteristics of high hardness, high strength, high elastic deformation capacity and good wear resistance, which are particularly suitable as brazing materials.

[0004] Ni-based amorphous alloy solder has advantages that traditional crystalline solders do not have, such as good thin strip formability, high toughness, strong processability, uniform solder composition and high designability. It has been widely used in the brazing connection of complex components of metal materials used in high-temperature applications such as high-temperature alloys and stainless steel. In order to reduce the melting point of Ni-based amorphous alloy solder, melting-reducing elements such as Si, P and B are usually added to it. Such additions can also improve the wetting and fluidity of the solder. However, during the brazing process of such materials, a variety of melting-reducing elements will generate a large amount of hard and brittle intermetallic compounds in the joint, which seriously affects the mechanical and corrosion resistance of the joint. In addition, in order to avoid the problem that the melting point and liquidus temperature of the solder alloy are too high and are not conducive to subsequent welding, refractory elements with ultra-high melting points, such as W, Mo, etc., are usually not introduced into the solder in large quantities. However, these refractory elements are usually used in large quantities as high-temperature solid solution strengthening elements in Ni-based high-temperature alloy brazing parent materials. Welded joints using brazing materials lacking these refractory elements often exhibit poor mechanical properties at room temperature or even at high temperatures, which seriously affects the reliability of related welding hot end components during use. In addition, the influence of alloy components on amorphous forming ability is very sensitive. The introduction of high-melting-point refractory elements will greatly reduce the amorphous forming ability of the alloy. Therefore, the development of such Ni-based amorphous alloy brazing materials containing refractory elements is usually extremely difficult.

[0005] In summary, the development of a new high-performance Ni-based amorphous alloy brazing material with a high content of refractory elements and a suitable melting point has important component design guidance significance and practical application value in the field of high-temperature alloy brazing connection technology. Summary of the invention

[0006] The purpose of the present invention is to provide a nickel-based amorphous alloy brazing material with a high W content, which solves the problem in the prior art that it is difficult to use refractory metals with a high melting point as welding materials. In the present invention, the constraints of the existing amorphous alloy brazing materials are broken through, and a new type of ternary and pseudo-ternary nickel-based amorphous alloy brazing materials with high W content, low melting point and high brazing joint strength are obtained, which can be used for high-quality nickel-based high-temperature alloy brazing connections.

[0007] To achieve the above object, the present invention provides a nickel-based amorphous alloy brazing material with a high W content, wherein the composition of the brazing material is generally Ni a Cr x W b B c , wherein a, x, b, and c all represent atomic percentages; and 0≤x≤10, 5≤b≤17.5, 15≤c≤22.5, a=100-xbc.

[0008] In the prior art, traditional Ni-based amorphous alloy solders rarely introduce a large amount of high-melting-point W elements, because the introduction of a large proportion of such elements may cause a significant increase in the melting point of the alloy, thereby reducing the ability to form amorphous alloys and making it impossible to prepare solders of corresponding components. In particular, the melting point of W is as high as 3620°C. Adding a large amount of W to the solder will cause a sharp increase in the melting point and liquidus of the alloy, which may cause a significant decrease in the amorphous forming ability of the alloy, so that the corresponding amorphous alloy solder cannot be prepared using the current rapid solidification technology.

[0009] In order to break through the constraints of existing amorphous alloy solder components, the present invention adopts the introduction of melting-reducing elements to improve this problem. When selecting melting-reducing elements, it is considered that B atoms are smaller in size than Si atoms and have a fast diffusion rate in Ni-based alloys, so they are easy to diffuse from the solder to the base material during the brazing process, and are not easy to form large-sized continuous brittle intermetallic compound phases. Therefore, the B element is introduced.

[0010] At the same time, as one of the melting point-reducing elements of Ni-based amorphous alloy solder, B element, when its content in the solder alloy is too high, will lead to the formation of a large number of intermetallic compounds in the joint, thus directly damaging the comprehensive performance of the joint; when the B element in the solder is too low, the liquidus temperature of the alloy will be too high, thus affecting the brazing process and even making it impossible to make the corresponding amorphous alloy solder. Therefore, it is necessary to accurately design the amount of B element. If possible, it is also possible to find an optimized component with a suitable liquidus temperature and a certain amorphous forming ability in the Ni-WB ternary system.

[0011] Based on this, in order to reduce the influence of the brazing thermal cycle on the base material, and considering that the Cr element has the ability to improve the anti-oxidation ability of the brazing seam. The present invention adopts the method of similar element replacement in the ternary NiWB system, and adopts the Cr element to replace the Ni element to obtain the quaternary Ni-Cr-WB amorphous alloy solder component, so as to further reduce the influence of the W element on the N-based amorphous alloy solder, thereby developing the core solution to be protected by the present invention, namely, two high W content, low melting point amorphous alloy solder component designs. The above-mentioned single element mainly plays the following roles in the present invention:

[0012] B: Reduce the melting point of solder and increase the amorphous forming ability of nickel-based amorphous alloy solder.

[0013] W: It plays a role of solid solution strengthening and helps to improve the room temperature and high temperature mechanical properties of the welded joint.

[0014] Cr: Lowers the liquidus temperature of the solder and helps improve the corrosion and oxidation resistance of the welded joint.

[0015] In a preferred embodiment, when the component of the brazing material is Ni 75 W5B 20When the melting point is detected, it is 1095-1120°C.

[0016] In a preferred embodiment, when the component of the brazing material is Ni 65 Cr 10 W5B 20 When the melting point is detected, it is 1045-1077°C.

[0017] It can be seen that the nickel-based amorphous alloy brazing material obtained by the present invention has the advantages of high W content and low melting point.

[0018] Another object of the present invention is to provide a method for preparing a nickel-based amorphous alloy brazing material with a high W content, wherein a master alloy ingot is obtained by a high-frequency induction melting method, and then a melt spinning method is used to stably obtain an amorphous alloy thin strip with a thickness of 30-70 μm and a width of 10 mm or more by adjusting the copper wheel speed and the injection pressure. Moreover, the obtained non-alloy and thin strip can also be prepared into a high-purity powdered brazing material or other forms of use by means such as mechanical grinding, which expands its application scenarios.

[0019] To achieve the above object, the present invention provides a method for preparing a nickel-based amorphous alloy brazing material with a high W content, which specifically comprises the following steps:

[0020] (1) According to the composition of the brazing material, convert the atomic percentage into mass percentage and accurately weigh Ni, W, B, and Cr as raw materials;

[0021] (2) placing raw materials in a vacuum high-frequency induction melting furnace in turn, evacuating the furnace and filling it with argon as a protective gas, and heating the furnace with a high-frequency power supply to obtain a master alloy ingot with uniform composition;

[0022] (3) After the master alloy ingot is crushed, an amorphous alloy solder strip with a thickness of 30-70 μm and a width of ≥10 mm is obtained by a rapid solidification method of melt spinning quenching.

[0023] In a preferred embodiment, in step (1), the purity of the Ni, W, B, and Cr single-substance raw materials used is 99.5% (mass ratio) or more.

[0024] In a preferred embodiment, in step (2), the order of placing the raw materials is to uniformly add B element first and then add Ni element last. Because the density of B element is relatively small, it needs to be placed in the smallest layer of the mixture, and all B element is added first; and Ni element is easier to melt, so it is added last to cover the surface. In addition, the metalloid B element is added in the present invention, which is a brittle material and has a large anisotropy in its thermal expansion coefficient. Direct arc melting will cause splashing, thereby affecting the accuracy of the alloy composition. Therefore, vacuum induction melting method is required for preparation.

[0025] In a preferred embodiment, in step (2), the vacuum condition is 5×10 -2 Pa, fill with 0.05Mpa argon gas.

[0026] In a preferred embodiment, in step (3), the rapid solidification method of melt spinning quenching is specifically as follows: placing the crushed master alloy in a quartz tube and assembling it in an extremely cold solidification device, adjusting the distance between the quartz tube nozzle and the copper wheel surface to 1-1.5 mm; evacuating the device and filling it with argon; using an induction coil to heat the master alloy to about 150° C. above its melting point, after the crushed alloy is completely turned into liquid and the surface fluctuates, immediately using a spray device to spray the hot melt onto the rotating copper wheel, and obtaining an amorphous alloy ribbon through rapid cooling; preferably, the quartz tube outlet width is more than 10 mm; preferably, the vacuum condition is 5×10 -2 Pa or less, and 0.05Mpa of argon is filled in; preferably, the injection pressure in the injection device is 0.03-0.06MPa, the gas stripping pressure is 0.02-0.04MPa, and the copper wheel speed is 2000-3000rpm; more preferably, the protective gas used in the smelting step, the injection gas used in the melt quenching step and the stripping gas are all high-purity argon.

[0027] Another object of the present invention is to provide an application of a nickel-based amorphous alloy brazing material with a high W content. The amorphous alloy brazing material prepared by any of the aforementioned methods can fully diffuse the B element in the brazing area of ​​the parent material to be welded by controlling the brazing time and the brazing temperature, thereby avoiding the formation of intermetallic compounds and forming a single W element solid solution structure, which plays a good role in strengthening and toughening the joint. The room temperature and high temperature mechanical properties of the obtained joint can reach more than 80% of the parent material, and can be used for high-quality nickel-based high-temperature alloy brazing connections.

[0028] To achieve the above object, the present invention provides an application of a nickel-based amorphous alloy brazing material with a high W content, which specifically comprises the following steps:

[0029] S1 Grind and clean the base metal to be welded to remove surface contaminants;

[0030] S2: Take the brazing material of claim 1 with a thickness of 30 μm and place it between two base materials to be welded, place it in a vacuum high-temperature brazing furnace, heat it up and braze it under vacuum, and cool it to room temperature after brazing.

[0031] In a preferred embodiment, in step S1, the grinding and cleaning can remove the contaminants on the surface of the base material that affect welding in a conventional manner known to those skilled in the art. The preferred grinding and cleaning method is: before brazing, the surface of the tissue sample is polished smooth using 360#, 800#, 1500# and 3000# SiC sandpapers on the base material to be welded, and the grinding direction is rotated 90° each time the sandpaper is changed. After grinding, the sample is polished with a diamond polishing agent, and then the sample is placed in ethanol for ultrasonic treatment for 15-25 minutes to remove the residual polishing agent and other stains on the surface, and finally the sample is blown dry with a hair dryer.

[0032] In a preferred embodiment, in step S2, the base material to be welded is GH3230 nickel-based deformable high-temperature alloy.

[0033] GH3230 alloy is a new type of Ni-Cr-W solid strengthening and carbide dispersion strengthening nickel-based high temperature alloy in China. The alloy has excellent high temperature mechanical properties, oxidation resistance and corrosion resistance, as well as good welding performance. In order to enable this type of material to be used for a long time under high temperature and stress environment, a large amount of Cr, W and Mo refractory elements and a small amount of C and B metal elements are added to the GH3230 alloy for alloying.

[0034] However, in the prior art, when brazing complex structural parts of GH3230 high-temperature alloy thin-walled plates, there are widespread problems that brittle intermetallic compound phases are easily formed in the joints and traditional crystalline alloy paste solder cannot achieve pre-laying of complex surfaces on narrow brazing seams. It is urgent to develop a new Ni-based amorphous alloy solder strip with both toughness and good brazing welding performance. The new high-performance Ni-based amorphous alloy solder provided by the present invention can achieve high-strength precision connection of GH3230 high-temperature alloys, which has important scientific research and industrial application value for the design and development of amorphous alloy solders and the independent production and manufacturing of my country's aero-engines.

[0035] In a preferred embodiment, in step S2, the vacuum degree in the vacuum state is 8×10 -3 Pa.

[0036] In a preferred embodiment, in step S2, the temperature-raising brazing conditions are: heating to 900-1000°C at a heating rate of 8-12°C / min and keeping warm for 8-10min; then heating to a welding temperature of 1140-1200°C at the original heating rate and brazing for 300-1800s. More preferably, the temperature-raising brazing conditions are: heating to 1000°C at a heating rate of 10°C / min and keeping warm for 10min; then heating to a welding temperature of 1180°C at the original heating rate and brazing for 1800s.

[0037] In a preferred embodiment, the brazing material is Ni75 W5B 20 The base material to be welded is GH3230, the welding temperature is 1180°C, the welding time is 1800s, and the obtained joint has a room temperature tensile strength of 860MPa and a high temperature tensile strength of 139MPa at 980°C.

[0038] Compared with the prior art, the technical solution of the present invention has the following advantages:

[0039] (I) The Ni-based ternary amorphous alloy material provided by the present invention has a wide composition range, wherein the atomic percentage of W can reach 5%-17.5%, and the atomic percentage of B is 15%-22.5%. Its optimal composition is Ni 75 W5B 20 It is the near-eutectic component with the lowest melting point in the ternary Ni-WB amorphous alloy, with a melting point of 1095-1120℃; the introduction of Cr element can further reduce the melting point of this type of pseudo-ternary alloy to 1045-1077℃, so that the amorphous alloy material can effectively reduce the melting point while maintaining a high W content.

[0040] (ii) The Ni-WB-(Cr) ternary and pseudo-ternary amorphous alloy solders provided by the present invention have good amorphous forming ability, and the critical size is not less than 35 μm.

[0041] (III) The melting point of the alloy-like solder prepared by the present invention is well suitable for the brazing connection of GH3230 high-temperature alloy, and the preparation method is simple and easy to operate. By optimizing and controlling the brazing time and the brazing temperature, the B element in the GH3230 brazing zone can be fully diffused to avoid the formation of intermetallic compounds and form a single W element solid solution structure, which plays a good role in joint strengthening and toughening. The room temperature and high temperature mechanical properties of the obtained joint can reach more than 80% of the parent material, and can be used for high-quality nickel-based high-temperature alloy brazing connection. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] These and / or other aspects and advantages of the present invention will become more clear and easier to understand from the following detailed description of the embodiments of the present invention in conjunction with the accompanying drawings, in which:

[0043] Figure 1 It is the X-ray diffraction (XRD) spectrum of the Ni-WB amorphous alloy solder sample in Examples 1-6 of the present invention.

[0044] Figure 2 It is the differential scanning calorimetry (DSC) curve of the Ni-WB amorphous alloy solder samples in Examples 1-6 of the present invention.

[0045] Figure 3 The Ni of different thicknesses in Example 2 of the present invention 75 W5B20 X-ray diffraction (XRD) patterns of the strip samples.

[0046] Figure 4 The Ni obtained by Example 2 of the present invention 75 W5B 20 Amorphous alloy brazing filler metal, brazing GH3230 alloy sample, element surface distribution diagram of the obtained joint (brazing conditions: 1180℃, 1800s).

[0047] Figure 5 The Ni obtained in Example 2 of the present invention 75 W5B 20 Amorphous alloy brazing filler metal, room temperature tensile strength of brazed joints at different brazing temperatures.

[0048] Figure 6 It is the differential scanning calorimetry (DSC) curve of the NiWB amorphous alloy solder and the Ni-Cr-WB amorphous alloy solder samples in Examples 2, 7 and 8 of the present invention.

[0049] Figure 7 is the Ni of different thicknesses in Example 7 of the present invention. 65 Cr 10 W5B 20 X-ray diffraction (XRD) patterns of the strip samples.

[0050] Figure 8 Ni obtained in Example 7 of the present invention 65 Cr 10 W5B 20 Amorphous alloy brazing filler metal, room temperature tensile strength of brazed joints at different brazing temperatures. DETAILED DESCRIPTION

[0051] In order to enable those skilled in the art to better understand the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods, but it should be understood that the protection scope of the present invention is not limited to the specific implementation methods.

[0052] The embodiments of the present invention provide a nickel-based amorphous alloy brazing material with a high W content and a preparation method and application thereof, thereby solving the problem in the prior art that high-melting-point refractory elements are used in the brazing material, resulting in a decrease in the mechanical properties of the welded joint and a decrease in the amorphous forming ability of the alloy.

[0053] The technical solution of the present application is described in detail below through specific embodiments:

[0054] Unless otherwise specified, the technical means used in the present invention are conventional means well known to those skilled in the art, and the various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. The reagents used in the present invention are analytically pure unless otherwise specified, the purity of the Ni and Cr single-substance raw materials used is 99.99%, the purity of the W single-substance raw material is 99.95%, the purity of the B single-substance raw material is 99.5%, and the purity of the argon used is 99.999%. The room temperature described in the present invention is 25°C.

[0055] The welding base material used in the embodiment of the present invention is GH3230 high temperature alloy, and its main chemical composition is shown in Table 1:

[0056] Table 1

[0057] element Ni Cr W Mo Co Fe C Al Mn wt.% Bal 21.61 14.34 1.32 1.13 0.92 0.10 0.36 0.52

[0058] The vacuum high-frequency induction melting furnace used in the embodiment of the present invention is model NEW-M04C, manufactured by Nissin Giken, the rapid solidification equipment used is model NEW-A05, manufactured by Nissin Giken, and the vacuum high-temperature brazing furnace used is model VBF-80, manufactured by Huahai Zhongyi. The test instrument used in the embodiment of the present invention is X-ray diffraction: the instrument selected is the D / MAX-2500 X-ray diffractometer produced by Rigaku Corporation of Japan, thermal analysis: the model STA-449F3 high-temperature synchronous thermal analyzer produced by NETZSCH of Germany is used, and the crystallization and melting behavior of the solder are analyzed by differential scanning calorimetry (DSC) to obtain the characteristic temperature of the solder crystallization process, as well as the melting point and liquidus temperature of the melting process.

[0059] The present invention adopts tensile strength to evaluate the connection strength of the joint, and adopts the test standard in GBT 11363-2008 Welding Joint Strength Test Method. More than 3 tensile specimens obtained under each condition are processed to avoid invalid data caused by some accidental reasons.

[0060] (I) Preparation of NiWB amorphous alloy solder

[0061] Step 1: Prepare Ni, W, and B single substances in corresponding proportions as raw materials according to the corresponding components of the Ni-WB amorphous alloy in Table 2.

[0062] Step 2: Put the raw materials weighed in the first step into the vacuum induction melting equipment in sequence. The order of adding is: first evenly add B element to the bottom layer, and finally add Ni element; the vacuum condition is 5×10 -2Pa, fill in 0.05Mpa high-purity argon as a protective gas, and perform vacuum induction melting by high-frequency power heating. After the alloy is completely molten, keep it warm for 5 minutes. After the alloy is cooled with the furnace, take it out from the melting equipment to obtain the master alloy of the solder.

[0063] Step 3: The alloy obtained in the second step was mechanically crushed and placed in a quartz tube with an outlet width of 10 mm, and then placed in a rapid solidification device for melt spinning quenching. The distance between the quartz tube nozzle and the copper wheel surface was adjusted to 1 mm. The cavity of the rapid solidification device was evacuated to a vacuum degree of 5×10 -2 Pa, and then filled with 0.05MPa high-purity argon; adjust the copper wheel speed of the rapid solidification equipment to 2000rpm, the injection pressure to 0.035MPa, and the gas stripping pressure to 0.03MPa, where both the injection gas and the stripping gas are high-purity argon. Use an induction coil to heat the master alloy to about 150°C above the melting point. After the crushed alloy completely turns into liquid and the surface fluctuates, immediately use a spray device to spray the hot melt onto the rotating copper wheel, and obtain an alloy thin strip with a thickness of 35μm and a width of 10mm after rapid cooling.

[0064] Table 2 Composition of amorphous alloy solder in Examples 1-6 and data on melting point and liquidus temperature of the prepared solder

[0065]

[0066]

[0067] The amorphous alloy solders obtained in Examples 1-6 were characterized and analyzed, and the results were as follows:

[0068] Depend on Figure 1 It can be seen from the XRD patterns shown that there are no sharp crystal diffraction peaks in the X-ray diffraction patterns of the six NiWB alloy samples, but only diffuse scattering peaks of amorphous structures, indicating that the alloy solders obtained in Examples 1-6 are of amorphous structures.

[0069] Depend on Figure 2 The differential scanning calorimetry (DSC) curves shown in FIG. 1 show the liquidus temperature of the solder in Examples 1 to 6. 75 W5B 20 There is only one melting endothermic peak in the melting stage of the amorphous alloy strip, and the temperature range between the solidus (Tm) and the liquidus (Tl) is relatively narrow, indicating that the alloy is a component near the eutectic point. This type of alloy usually has good amorphous forming ability and good fluidity in the molten state, making it more suitable as a solder alloy.

[0070] Furthermore, the Ni 75 W5B20 When the amorphous alloy strips were used, the copper wheel speed in step 3 was adjusted to 2500 rpm and 3000 rpm, respectively, to obtain strip samples with thicknesses of 50 μm and 70 μm, respectively. 75 W5B 20 The X-ray diffraction pattern of the strip sample is as follows Figure 3 As shown. Figure 3 It can be seen that the thickness of Ni is 35um 75 W5B 20 The XRD spectrum of the strip sample only shows a single diffuse scattering peak near 2θ=44.5°. As the sample thickness increases and the cooling rate decreases during the preparation process, more crystal diffraction peaks appear in the XRD spectrum. 75 W5B 20 The critical size of amorphous alloys is about 35um.

[0071] (2), Ni 75 W5B 20 Application of amorphous alloy solder

[0072] The Ni prepared in Example 2 75 W5B 20 The amorphous alloy brazing material is used to braze the GH3230 alloy in a vacuum brazing furnace. The specific steps include:

[0073] Before S1 brazing, the surface of the tissue sample of the base material GH3230 alloy to be welded was polished smooth using 360#, 800#, 1500# and 3000# Si C sandpaper in turn. The grinding direction was rotated 90° each time the sandpaper was changed. After grinding, it was polished with diamond polishing agent, and then the sample was placed in ethanol for ultrasonic treatment for 25 minutes to remove the residual polishing agent and other stains on the surface. Finally, the sample was blown dry with a hair dryer.

[0074] S2 brazing joints are overlapped with Ni 75 W5B 20 For example, the amorphous alloy ribbon is pre-placed between two GH3230 alloy plates to form a sandwich structure. The brazing workpiece is placed in a vacuum brazing furnace. When the vacuum degree reaches 8.0×10 - 3 Pa, and then heated to 1000℃ at a rate of 10℃ / min, and kept warm for 10min, and then heated to different brazing temperatures (1140℃, 1160℃, 1180℃, 1200℃) at a rate of 10℃ / min, and kept warm for 30min. Then the heating system was turned off, and the brazed structure was cooled to room temperature with the furnace. After the brazed structure cooled to room temperature, it was taken out of the vacuum brazing furnace, its related mechanical properties were tested, and the organizational structure of the brazing seam area was analyzed. The results are as follows Figure 4 and Figure 5 shown.

[0075] Figure 4 For N i 75 W5B 20 Element surface distribution diagram of GH3230 brazed joint obtained by brazing amorphous alloy brazing material at a brazing temperature of 1180℃ and a brazing time of 30min. All B elements in the brazing seam area diffuse into the base material, and a relatively uniformly distributed flocculent precipitate phase is generated along the grain boundary at the far end of the diffusion zone. The W element mainly remains in the brazing seam area due to its large atomic size and slow diffusion rate. Using this high-W nickel-based amorphous alloy brazing material, under the conditions of optimized process parameters, no brittle intermetallic compound phase is generated in the brazing seam area, and a W element with uniform composition is dissolved in the γ phase continuous solid solution.

[0076] Figure 5 This shows that the brazing temperature has an effect on the use of Ni 75 W5B 20 The influence of amorphous alloy brazing filler metal on the room temperature tensile strength of the joint obtained by brazing GH3230. Figure 5 It can be seen that the room temperature tensile strength of the joint increases first and then decreases with the increase of brazing temperature, which is basically equivalent to the strength of the parent material. When the brazing temperature is 1180℃, the boride in the brazing seam area disappears, the joint is homogenized, the room temperature tensile strength reaches a maximum of 860MPa, and most of the specimen fractures occur in the parent material part. In addition, the GH3230 high temperature alloy is mainly used in high temperature environments, and the high temperature mechanical properties of the joint need to be evaluated. The present invention selects the brazing process parameters with the best room temperature tensile strength, that is, the brazing temperature is 1180℃, and the brazing time is 1800s. The joint is subjected to a high temperature tensile test under a 980℃ environment. The results show that the high temperature tensile strength of the brazed joint at 980℃ is 139MPa (about 92% of the high temperature tensile strength of the GH3230 high temperature alloy parent material at the corresponding temperature). It can be seen that the brazing material obtained by the present invention has good high temperature performance, and its high temperature mechanical properties are also equivalent to the corresponding parent material.

[0077] (III) Preparation of Ni-Cr-WB amorphous alloy solder

[0078] Step 1: Prepare corresponding proportions of Ni, Cr, W, and B as raw materials according to the corresponding components of the Ni-Cr-WB amorphous alloy in Table 3.

[0079] The remaining steps are completely consistent with the equipment and parameter design used to prepare Ni-WB amorphous alloy solder.

[0080] Table 3 Composition of amorphous alloy solder in Examples 7-8 and data on melting point and liquidus temperature of the prepared solder

[0081]

[0082] The amorphous alloy solder obtained in Examples 7-8 was characterized and analyzed, and the results were as follows:

[0083] In order to further reduce the brazing temperature as much as possible, the inventors tried to add Cr element to the NiWB ternary system in order to reduce the melting point of the brazing material and improve the oxidation resistance of the brazing seam. Based on this, Examples 7 and 8 respectively replaced Ni in Example 1 with 5 and 10 atomic percent of Cr element. 75 W5B 20 The melting DSC curve of the Ni element in the alloy is as follows: Figure 6 The solidus temperature (melting point) and liquidus temperature of the corresponding alloy are shown in Table 3. It can be seen that replacing Ni with Cr 75 W5B 20 After the Ni element is added, the solidus and liquidus temperatures of the alloy decrease with the increase of Cr content, and the melting endothermic peak of the quaternary Ni-Cr-WB alloy is only one. Compared with the ternary alloy, the quaternary Ni-Cr-WB alloy obtained by replacing the Ni element with 10 atomic percent of Cr is 65 Cr 10 W5B 20 The liquidus temperature of the alloy drops to 1077℃ at its lowest.

[0084] Similarly, the inventors prepared Ni 65 Cr 10 W5B 20 When soldering amorphous alloy, the copper wheel speed in step 3 was adjusted from 2000rpm to 2500rpm and 3000rpm. On the basis of the original thickness of 35μm, strip samples with thickness of 50μm and 70μm were obtained respectively. The results of Ni 65 Cr 10 W5B 20 The X-ray diffraction pattern of the strip sample is as follows Figure 7 As shown in the figure, the XRD patterns of the strips with thickness of 35 mm and 50 mm both show the characteristics of the X-ray diffraction patterns of typical amorphous alloys. When the cooling rate is further reduced during the solidification of the alloy, the crystal phase of Ni appears in the strip with a thickness of 70 mm. Therefore, Ni 65 Cr 10 W5B 20 The critical size of the amorphous alloy is about 50 μm, which shows that the introduction of Cr, a similar element to Ni, can significantly improve the amorphous forming ability of the alloy.

[0085] Under different brazing temperature conditions, the 65 Cr 10 W5B20 The room temperature tensile strength evaluation of the joints obtained by brazing GH3230 with amorphous alloy brazing filler metals shows that when the brazing temperature is 1200℃, the room temperature tensile strength is the highest, reaching 783MPa.

[0086] (4), Ni 65 Cr 10 W5B 20 Application of amorphous alloy solder

[0087] Adopt (II), Ni 75 W5B 20 In the application of amorphous alloy brazing materials, the GH3230 alloy was brazed with exactly the same welding method, and its related mechanical properties were tested. The results are as follows: Figure 8 shown.

[0088] Figure 8 The effect of brazing temperature on the Ni 65 Cr 10 W5B 20 The influence of amorphous alloy brazing filler metal on the room temperature tensile strength of the joint obtained by brazing GH3230. It can be seen from the figure that the room temperature tensile strength of the joint increases with the increase of brazing temperature. The room temperature tensile strength of the joint obtained when the brazing temperature is 1140℃ is the lowest. The large amount of W-rich borides in the brazing seam area seriously reduces the mechanical properties of the joint, and the room temperature tensile strength of the joint is only 565MPa. When the brazing temperature rises to 1200℃, the amount of W-rich borides in the brazing seam area decreases, and the room temperature tensile strength is the highest, reaching 783Mpa.

[0089] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.

Claims

1. A method for preparing a nickel-based amorphous alloy brazing material with a high W content, characterized in that: The general formula of the brazing material is Ni a W b B c , wherein a, b, and c all represent atomic percentages; and b=5, c=20, a=100-bc, and the melting point of the brazing material is 1095-1120°C; The specific steps include: (1) According to the composition of the brazing material, convert the atomic percentage into mass percentage and accurately weigh Ni, W, and B as raw materials; (2) placing raw materials in a vacuum high-frequency induction melting furnace in turn, evacuating the furnace and filling it with argon as a protective gas, and heating the furnace with a high-frequency power supply to obtain a master alloy ingot with uniform composition; (3) After the master alloy ingot is crushed, an amorphous alloy solder strip with a thickness of 30-70 μm and a width of ≥10 mm is obtained by a rapid solidification method of melt spinning quenching; In step (2), the order of placing the raw materials is to uniformly add the B element first and then add the Ni element last.

2. The method for preparing a nickel-based amorphous alloy brazing material with a high W content according to claim 1, characterized in that: In step (3), the rapid solidification method of melt spinning quenching is specifically as follows: the crushed master alloy is placed in a quartz tube and assembled in an extremely cold solidification device, and the distance between the quartz tube nozzle and the copper wheel surface is adjusted to be 1-1.5 mm; the device is evacuated and filled with argon; the injection pressure is adjusted to 0.03-0.06MPa and the copper wheel speed is adjusted to 2000-3000rpm, and the superheated melt is sprayed onto the rotating copper wheel, and cooled.

3. The use of the nickel-based amorphous alloy brazing material with high W content as claimed in claim 1, characterized in that: The following steps are involved: S1 Grind and clean the base metal to be welded to remove surface contaminants; S2: Take the brazing material of claim 1 with a thickness of 30 μm and place it between two base materials to be welded, place it in a vacuum high-temperature brazing furnace, heat it up and braze it under vacuum, and cool it to room temperature after brazing.

4. The use of the nickel-based amorphous alloy brazing material with high W content as claimed in claim 3, characterized in that: In step S1, the base material to be welded is GH3230 nickel-based deformable high-temperature alloy.

5. The use of the nickel-based amorphous alloy brazing material with high W content as claimed in claim 3, characterized in that: In step S2, the temperature-raising brazing conditions are: heating to 900-1000°C at a heating rate of 8-12°C / min and keeping warm for 8-10min; then heating to a welding temperature of 1140-1200°C at the original heating rate and brazing for 300-1800s.

6. The use of the nickel-based amorphous alloy brazing material with high W content as claimed in claim 5, characterized in that: The brazing material is Ni 75 W5B 20 The base material to be welded is GH3230, the welding temperature is 1180°C, the welding time is 1800s, and the obtained joint has a room temperature tensile strength of 860MPa and a high temperature tensile strength of 139MPa at 980°C.