Plastic steel PPS composite material and preparation process thereof

Through the design of composite filler composition and hyperbranched PPS resin combined with built-in aramid fiber-based woven fabric, the problem of insufficient impact toughness of polyphenylene sulfide composite material is solved, and the multiple properties of plastic steel PPS composite material are improved to meet the requirements of Protection needs for lithium battery case of new energy vehicles.

CN119058196AActive Publication Date: 2024-12-03浙江荣泰电工器材股份有限公司

Patent Information

Application Number
CN202411436908.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-03
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

The existing high-performance polyphenylene sulfide composite materials have insufficient impact toughness in the field of lithium batteries in new energy vehicles and cannot meet the protection needs of battery shell materials.

Method used

The composite design of composite filler composition and hyperbranched PPS resin combined with built-in aramid fiber-based woven fabric is optimized to optimize the ratio of spherical, fibrous and sheet-shaped fillers, and improve the mechanical strength and thermal stability of plastic steel PPS composite materials. Chemical corrosion resistance, electrical properties and impact toughness.

Benefits of technology

The overall performance improvement of plastic steel PPS composite materials has been achieved, meeting the needs of battery shell materials, including improving mechanical strength, thermal stability, chemical corrosion resistance, electrical properties and impact toughness, and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of plastic steel composite materials for new energy automobiles, in particular to a plastic steel PPS composite material and a preparation process thereof. The plastic steel PPS composite material comprises modified PPS matrix resin and at least one piece of aramid fiber-based woven fabric compounded in the modified PPS matrix resin, the aramid fiber-based woven fabric is of a warp and weft knitted structure of a plain weave structure, warps in the aramid fiber-based woven fabric at least comprise aramid fibers, and wefts in the aramid fiber-based woven fabric at least comprise aramid fibers; the modified PPS matrix resin is prepared from the following raw materials in parts by mass: 100 parts of PPS resin, 5-20 parts of hyperbranched PPS resin, 50-70 parts of a filler composition, 0.5-2 parts of a dispersing agent and 1-3 parts of an anti-aging agent. The material has good thermal stability, chemical corrosion resistance, electrical properties, wear resistance and flame retardance, also has good impact toughness and mechanical strength, and can meet the use requirements of battery shell materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of preparation of plastic-steel composite materials for new energy vehicles, and in particular to a plastic-steel PPS composite material and a preparation process thereof. Background Art

[0002] Polyphenylene sulfide has excellent mechanical properties, thermal stability, chemical corrosion resistance, electrical properties, wear resistance and flame retardancy, and has been used in lithium batteries, lightweight vehicles, aviation materials, organic matter treatment in sewage and other fields. At present, polyphenylene sulfide is widely used in the automotive field in igniters, connectors, thermostats, IGBT modules, heater brackets, generator coil skeletons and other automotive parts. With the rapid development of new energy vehicles, polyphenylene sulfide has been developed and applied in the peripheral components of new energy vehicle drive motors and power batteries. For example, the lithium battery brackets in some high-end models are made of polyphenylene sulfide composite materials.

[0003] Due to the shortcomings of high crystallinity and brittleness of polyphenylene sulfide, it is impossible to prepare high-toughness polyphenylene sulfide products. At the same time, the high melting point of polyphenylene sulfide reduces its fluidity during melt processing, resulting in deviations in the overall processing performance, making it impossible to produce and process special-shaped structural parts around new energy vehicle drive motors and power batteries.

[0004] For example, the battery shell of lithium batteries used to be made of 304 or 306 stainless steel with good rust and corrosion resistance. With the increasing requirements for lightweight vehicles, rust-resistant and corrosion-resistant 3003 aluminum alloy materials are gradually replacing 304 or 306 stainless steel as the battery shell of lithium batteries, providing good protection and support for lithium battery modules. The density of 3003 aluminum alloy material is 2.70±0.02g / cm 3 , tensile strength σ b The material has a conditional yield strength of 140-180 MPa and a conditional yield strength of σ0.2 ≥ 85 MPa. It has good plasticity and anti-rust and corrosion properties and is suitable for battery casing materials.

[0005] With the increasing demand for lightweight vehicles, automakers want to find a high-performance polymer plastic-steel composite material to replace 3003 aluminum alloy battery shell materials. The excellent performance of polyphenylene sulfide has attracted the attention of the new energy industry: the density of the 40wt% GF modified polyphenylene sulfide material is currently publicized at 1.55-1.72 g / cm 3, it has good lightweight advantages and its tensile properties also meet the requirements. Its tensile strength is 135-220 MPa and its bending strength is 200-300 MPa. However, its strength is high and its impact toughness is biased. As a battery shell, it is easily brittle due to external impact. Its protection performance is questioned, which limits its application in new energy vehicle battery modules. In summary, although the existing high-performance polyphenylene sulfide composite materials have the advantages of lightweight and mechanical strength in the field of lithium batteries for new energy vehicles, their impact toughness is relatively general and cannot meet the protection requirements of battery shell materials. To this end, the present application provides a plastic-steel PPS composite material and a preparation process thereof. Summary of the invention

[0006] In order to solve the above-mentioned problems in the prior art, the present application provides a plastic-steel PPS composite material and a preparation process thereof.

[0007] The plastic-steel PPS composite material provided in this application is realized by the following technical solutions: A plastic-steel PPS composite material, comprising a modified PPS matrix resin and at least one aramid fiber-based woven fabric compounded inside the modified PPS matrix resin, wherein the aramid fiber-based woven fabric is a warp-weft knitted structure of a plain weave structure, wherein the warp threads of the aramid fiber-based woven fabric at least include aramid fibers, and the weft threads at least include aramid fibers; The modified PPS matrix resin is made of the following raw materials in parts by mass: 100 parts of PPS resin, 5-20 parts of hyperbranched PPS resin, 50-70 parts of filler composition, 0.5-2 parts of dispersant, and 1-3 parts of anti-aging agent; The dispersant is at least one of stearate, siloxane coupling agent and titanate coupling agent; The anti-aging agent is at least one of antioxidant 1024, antioxidant 4426, antioxidant 300, antioxidant 168, and antioxidant 626; The filler composition comprises a combination of spherical fillers, fibrous fillers and flake fillers. The spherical filler includes at least one of spherical alumina, spherical aluminum nitride, spherical silicon dioxide, spherical silicon nitride, spherical titanium nitride, and spherical silicon carbide; The fibrous filler comprises at least one of nanocarbon fibers, chopped aramid fiber compositions, carbon nanotubes, cellulose nanofibers, and inorganic whiskers; The inorganic whiskers include at least one of zinc oxide whiskers, aluminum oxide whiskers, zirconium oxide whiskers, aluminum nitride whiskers, boron nitride whiskers, silicon dioxide whiskers, silicon nitride whiskers, silicon carbide whiskers, calcium carbonate whiskers, and potassium titanate whiskers; The flaky filler includes at least one of graphene nanosheets, boron nitride nanosheets, MXene phase ceramic nanosheets, ultrafine mica sheets, and molybdenum sulfide nanosheets.

[0008] The composite design of the compound filler composition and the hyperbranched PPS resin combined with the built-in aramid fiber-based woven fabric in this application effectively improves the overall mechanical strength, thermal stability, chemical corrosion resistance, electrical properties, wear resistance and flame retardancy of the plastic-steel PPS composite material, and at the same time has excellent impact toughness, meeting the requirements of battery shell materials.

[0009] Preferably, the mass ratio of the spherical filler, the fibrous filler and the flake filler is (50-80):(10-30):(10-20).

[0010] The overall mechanical strength can be improved by optimizing the ratio of spherical fillers, fibrous fillers and flake fillers.

[0011] Preferably, the spherical filler is spherical alumina, spherical silicon nitride, and spherical titanium nitride in a mass ratio of (80-90):(5-10):(5-10); the spherical alumina is composed of nano-spherical alumina with an average particle size of 100-400nm, ultrafine spherical alumina with an average particle size of 0.5-5 μm, and spherical alumina with an average particle size of 25-50 μm in a mass ratio of (15-25):(35-60):(25-40); the average particle size of the spherical silicon nitride is 0.8-5 μm; and the average particle size of the spherical titanium nitride is 0.02-5 μm.

[0012] Preferably, the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers; the mass ratio of the chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers is (40-73):(25-50):(1-5):(1-5).

[0013] Preferably, the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets and ultrafine mica sheets; the mass ratio of the molybdenum sulfide nanosheets, boron nitride nanosheets and ultrafine mica sheets is (5-20):(5-20):(60-90).

[0014] By adopting the above technical solution, the overall mechanical strength can be further improved, and it is also beneficial to enhance the impact toughness, thermal stability, chemical corrosion resistance, electrical properties, wear resistance and flame retardancy.

[0015] Preferably, the ultrafine mica sheet is a surface carbon nanotube grafted modified mica sheet and / or a surface graphene grafted modified mica sheet; the surface carbon nanotube grafted modified mica sheet comprises an ultrafine mica sheet carrier with a particle size of ≤1250 mesh and carbon nanotubes fixed to the ultrafine mica sheet carrier with a particle size of ≤1250 mesh by nanosilver sintering; the surface graphene grafted modified mica sheet comprises an ultrafine mica sheet carrier with a particle size of ≤1250 mesh and graphene nanosheets fixed to the ultrafine mica sheet carrier with a particle size of ≤1250 mesh by nanosilver sintering.

[0016] By adopting the above technical solution, the overall mechanical strength and insulation and thermal conductivity can be further improved.

[0017] Preferably, the mass ratio of the spherical filler, the fibrous filler and the flaky filler is (55-60):(20-25):(15-20); the dispersant is composed of KH-550 silane coupling agent, KH-570 silane coupling agent and titanate coupling agent HY-311 in a mass ratio of (0.5-2):(0.5-2):(0.1-0.4).

[0018] By adopting the above technical solution, the overall mechanical strength and impact toughness can be further improved.

[0019] Preferably, the aramid fiber-based woven fabric is a plain weave warp and weft knitted structure, with the spacing between adjacent warps being 0.5-2 mm; the spacing between adjacent wefts being 0.5-2 mm; the warps in the aramid fiber-based woven fabric include aramid fiber filaments and carbon fiber filaments arranged at intervals from each other; the wefts in the aramid fiber-based woven fabric include aramid fiber filaments and carbon fiber filaments arranged at intervals from each other.

[0020] Preferably, the aramid fiber-based woven fabric needs to be subjected to a surface modification process before use; the surface modification process of the aramid fiber-based woven fabric is as follows: Step 1: the aramid fiber-based woven fabric is ultrasonically cleaned in an ethanol aqueous solution, then rinsed with clean water, dried, and set aside; Step 2, treating the aramid fiber-based woven fabric with low-temperature plasma, first with ozone at 0-4°C for 60-300s, and then with ammonia at 0-4°C for 60-300s, to obtain a semi-finished aramid fiber-based woven fabric; Step three, placing the aramid fiber-based woven fabric that has completed the low-temperature plasma treatment in a methacryloxysilane aqueous solution, heating it to 45-50°C for ultrasonic dispersion treatment for 20-40 minutes, wherein the methacryloxysilane concentration in the methacryloxysilane aqueous solution is 4-8wt%. After completing the ultrasonic dispersion treatment, take out the aramid fiber-based woven fabric, drain it and dry it to obtain the finished aramid fiber-based woven fabric.

[0021] By adopting the above technical scheme, the interfacial compatibility between aramid fiber-based woven fabric and modified PPS matrix resin is improved, which is beneficial to the improvement of mechanical strength, impact toughness, thermal stability, chemical corrosion resistance, electrical properties, wear resistance and flame retardancy.

[0022] The preparation process of a plastic-steel PPS composite material provided in this application is achieved through the following technical solutions: A preparation process of a plastic-steel PPS composite material comprises the following steps: Step 1, first prepare a filler composition, and then perform surface modification treatment on the prepared filler composition: place the filler composition in a surface modification liquid for ultrasonic dispersion treatment for 20-40 minutes, drain and dry to obtain a finished filler composition; the surface modification liquid is composed of a surface modifier and deionized water, and the surface modifier is a siloxane coupling agent and / or a titanate coupling agent; At the same time, the aramid fiber-based woven fabric is subjected to a surface modification process to obtain a finished aramid fiber-based woven fabric; Step 2, the filler composition in step 1 is mixed and dispersed uniformly with the correctly measured PPS resin, hyperbranched PPS resin, dispersant and anti-aging agent at high speed, and then put into a twin-screw extruder, and melt-extruded, wire-drawn, nitrogen-cooled, granulated and dried at a barrel end temperature of 285-325° C. to obtain a PPS composite masterbatch; Step 3, using PPS composite masterbatch for injection molding to form a PPS sheet with a thickness of 0.25-0.40 mm; Step 4: stacking to form a PPS sheet / finished aramid fiber-based woven fabric / PPS sheet structure, hot pressing at 280-300°C and 5-15MPa for 5-15min to obtain a PPS composite sheet, heat treating the obtained PPS composite sheet at 140-160°C for 30-60min, and naturally cooling to room temperature to obtain a plastic-steel PPS composite sheet that meets the use requirements of battery shell materials.

[0023] The preparation process of the present application improves the processing performance of PPS and the implementation scheme is relatively simple, which facilitates industrial production.

[0024] In summary, this application has the following advantages: 1. The composite design of the compound filler composition and the hyperbranched PPS resin combined with the built-in aramid fiber-based woven fabric in this application effectively improves the overall mechanical strength, thermal stability, chemical corrosion resistance, electrical properties, wear resistance and flame retardancy of the plastic-steel PPS composite material, and at the same time has excellent impact toughness, meeting the requirements of battery shell materials.

[0025] 2. In this application, the filler composition formed by optimizing the ratio of spherical fillers, fibrous fillers, and flaky fillers reduces the amount of the filler composition while ensuring the same physical and chemical properties of the plastic-steel PPS composite board, which is beneficial to reducing the overall production cost.

[0026] 3. The preparation process of the present application improves the processing performance of PPS and the implementation scheme is relatively simple, which facilitates industrial production. DETAILED DESCRIPTION

[0027] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and comparative examples. Example

[0028] A plastic-steel PPS composite material includes a modified PPS matrix resin and at least one aramid fiber-based woven fabric compounded inside the modified PPS matrix resin. The aramid fiber-based woven fabric is a warp-weft knitted structure of a plain weave structure, and the warp threads in the aramid fiber-based woven fabric at least include aramid fibers, and the weft threads at least include aramid fibers.

[0029] The modified PPS matrix resin comprises the following raw materials in parts by weight: 100 parts of PPS resin, 5-20 parts of hyperbranched PPS resin, 50-70 parts of filler composition, 0.5-2 parts of dispersant, and 1-3 parts of anti-aging agent.

[0030] Preferably, the modified PPS matrix resin is made of the following raw materials in parts by mass: 100 parts of PPS resin, 15 parts of hyperbranched PPS resin, 65 parts of filler composition, 2 parts of dispersant, and 3 parts of anti-aging agent.

[0031] The dispersant is at least one of stearate, siloxane coupling agent and titanate coupling agent.

[0032] Preferably, the mass ratio of spherical filler, fibrous filler and flake filler is (50-80):(10-30):(10-20).

[0033] Preferably, the mass ratio of spherical filler, fibrous filler and flake filler is (55-60):(20-25):(15-20).

[0034] Preferably, the dispersant is composed of KH-550 silane coupling agent, KH-570 silane coupling agent, and titanate coupling agent HY-311 in a mass ratio of (0.5-2):(0.5-2):(0.1-0.4).

[0035] The anti-aging agent is at least one of antioxidant 1024, antioxidant 4426, antioxidant 300, antioxidant 168, and antioxidant 626. Preferably, the anti-aging agent is composed of antioxidant 1024 and antioxidant 168.

[0036] The filler composition comprises spherical fillers, fibrous fillers and flake fillers.

[0037] The spherical filler includes at least one of spherical alumina, spherical aluminum nitride, spherical silicon dioxide, spherical silicon nitride, spherical titanium nitride, and spherical silicon carbide. Preferably, the spherical filler is spherical alumina, spherical silicon nitride, and spherical titanium nitride in a mass ratio of (80-90): (5-10): (5-10). The spherical alumina is composed of nano-spherical alumina with an average particle size of 100-400nm, ultrafine spherical alumina with an average particle size of 0.5-5 μm, and spherical alumina with an average particle size of 25-50 μm in a mass ratio of (15-25): (35-60): (25-40). The average particle size of spherical silicon nitride is 0.8-5 μm. The average particle size of spherical titanium nitride is 0.02-5 μm.

[0038] The inorganic whiskers include at least one of zinc oxide whiskers, aluminum oxide whiskers, zirconium oxide, aluminum nitride whiskers, boron nitride whiskers, silicon dioxide whiskers, silicon nitride whiskers, silicon carbide whiskers, calcium carbonate whiskers, and potassium titanate whiskers. Preferably, the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers, and the mass ratio of the chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers is (40-73):(25-50):(1-5):(1-5).

[0039] The flaky filler includes at least one of graphene nanosheets, boron nitride nanosheets, MXene phase ceramic nanosheets, ultrafine mica sheets, and molybdenum sulfide nanosheets. Preferably, the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets, and the mass ratio of molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets is (5-20): (5-20): (60-90).

[0040] Preferably, the ultrafine mica flakes are mica flakes modified by surface grafting of carbon nanotubes and / or mica flakes modified by surface grafting of graphene.

[0041] The surface carbon nanotube grafted modified mica sheet comprises an ultrafine mica sheet carrier with a particle size of ≤1250 meshes and carbon nanotubes fixed on the ultrafine mica sheet carrier with a particle size of ≤1250 meshes through nano-silver sintering.

[0042] The surface graphene grafted modified mica sheet comprises an ultrafine mica sheet carrier with a particle size of ≤1250 meshes and a graphene nanosheet fixed on the ultrafine mica sheet carrier with a particle size of ≤1250 meshes through nano-silver sintering.

[0043] The aramid fiber-based woven fabric is a plain weave structure with a warp-weft knitted structure, wherein the interval between adjacent warps is 0.5-2 mm and the interval between adjacent wefts is 0.5-2 mm. The warps in the aramid fiber-based woven fabric include aramid fiber filaments and carbon fiber filaments arranged at intervals from each other. The wefts in the aramid fiber-based woven fabric include aramid fiber filaments and carbon fiber filaments arranged at intervals from each other.

[0044] Aramid fiber-based woven fabrics need to undergo surface modification before use.

[0045] The surface modification process of aramid fiber-based woven fabric is as follows: Step 1: the aramid fiber-based woven fabric is ultrasonically cleaned in an ethanol aqueous solution, then rinsed with clean water, dried, and set aside; Step 2, treating the aramid fiber-based woven fabric with low-temperature plasma, first with ozone at 0-4°C for 60-300s, and then with ammonia at 0-4°C for 60-300s, to obtain a semi-finished aramid fiber-based woven fabric; Step 3: Place the aramid fiber-based woven fabric that has completed the low-temperature plasma treatment in a methacryloxysilane aqueous solution, heat it to 45-50°C and perform ultrasonic dispersion treatment for 20-40 minutes. The methacryloxysilane aqueous solution has a methacryloxysilane concentration of 4-8wt%. After the ultrasonic dispersion treatment, take out the aramid fiber-based woven fabric, drain it, and then dry it to obtain the finished aramid fiber-based woven fabric. A preparation process of a plastic-steel PPS composite material comprises the following steps: Step 1, first prepare a filler composition, and then perform surface modification treatment on the prepared filler composition: place the filler composition in a surface modification liquid for ultrasonic dispersion treatment for 20-40 minutes, drain and dry to obtain a finished filler composition; the surface modification liquid is composed of a surface modifier and deionized water, and the surface modifier is a siloxane coupling agent and / or a titanate coupling agent; At the same time, the aramid fiber-based woven fabric is subjected to a surface modification process to obtain a finished aramid fiber-based woven fabric; Step 2, the filler composition in step 1 is mixed and dispersed uniformly with the correctly measured PPS resin, hyperbranched PPS resin, dispersant and anti-aging agent at high speed, and then put into a twin-screw extruder, and melt-extruded, wire-drawn, nitrogen-cooled, granulated and dried at a barrel end temperature of 285-325° C. to obtain a PPS composite masterbatch; Step 3, using PPS composite masterbatch for injection molding to form a PPS sheet with a thickness of 0.25-0.40 mm; Step 4: stacking to form a PPS sheet / finished aramid fiber-based woven fabric / PPS sheet structure, hot pressing at 280-300°C and 5-15MPa for 5-15min to obtain a PPS composite sheet, heat treating the obtained PPS composite sheet at 140-160°C for 30-60min, and naturally cooling to room temperature to obtain a plastic-steel PPS composite sheet that meets the use requirements of battery shell materials.

[0046] Embodiment 1: A plastic-steel PPS composite material includes a modified PPS matrix resin and an aramid fiber-based woven fabric compounded inside the modified PPS matrix resin. The aramid fiber-based woven fabric is a warp-weft knitted structure of a plain weave, the warp is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn), and the interval between adjacent warps is 1mm; the weft is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn), and the interval between adjacent wefts is 1mm, that is, the aramid fiber-based woven fabric is formed with a 1mm*1mm mesh.

[0047] The modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin (Polyplastics of Japan, brand No. 0220A9, PPS pure resin, injection molding grade, melt viscosity of 260 Pa*s at 310°C), 5 parts of hyperbranched PPS resin, 50 parts of filler composition, 0.6 parts of dispersant K550 coupling agent, 0.6 parts of dispersant K570 coupling agent, 0.2 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0048] Preparation of hyperbranched PPS resin: Add 10g of 3,4-dichlorothiophenol, 3.4g of anhydrous potassium carbonate and 80mL of N-methylpyrrolidone to a 250mL three-necked bottle, heat to 150°C, and keep warm for 8.5h. Wash and filter the product with hydrochloric acid, add tetrahydrofuran to dissolve, extract with hexane, filter and dry to obtain light brown hyperbranched PPS powder.

[0049] The filler composition is composed of spherical fillers, fibrous fillers and flake fillers in a mass ratio of 60:20:20.

[0050] The spherical filler is composed of spherical alumina, spherical silicon nitride, and spherical titanium nitride in a mass ratio of 80:10:10. The spherical alumina is composed of nano-spherical alumina with an average particle size of 300nm (Jinzhong New Materials SINA-PROSPER, E300-1 nano-spherical alumina), ultrafine spherical alumina with an average particle size of 3±1μm (Wuhu Xinda New Materials Technology Co., Ltd., XD-LA03R), and spherical alumina with an average particle size of 30±3μm (Wuhu Xinda New Materials Technology Co., Ltd., XD-LA30R) in a mass ratio of 15:60:25.

[0051] The average particle size of spherical silicon nitride is 3-5 μm, and Nangong Rongbang New Material Technology Co., Ltd. customizes the particle size to be 3-5 μm.

[0052] The average particle size of spherical titanium nitride is 2 μm, brand is Zhongke Yannuo, scientific research grade.

[0053] The fibrous filler is composed of a chopped aramid fiber composite, single-walled carbon nanotubes (CNT200 Zhongke Leiming, tube diameter 1-2nm, length 5-30μm), zinc oxide whiskers (tetra-needle zinc oxide whiskers, XD-7.JX05, diameter 0.5-5μm, length 10-50μm, Wuhu Xinda New Material Technology Co., Ltd.), and potassium titanate whiskers (diameter 0.3-0.5μm, length 5-40μm, Wuhan Lanabai Pharmaceutical Chemical Co., Ltd.) in a mass ratio of 70:25:2:3.

[0054] The chopped aramid fiber composition is composed of DuPont Teijin para-aramid chopped PPTA with an equivalent diameter of 1 μm and a length of 0.5 mm, DuPont Teijin para-aramid chopped PPTA with an equivalent diameter of 1 μm and a length of 1 mm, DuPont Teijin para-aramid chopped PPTA with an equivalent diameter of 1 μm and a length of 3 mm, DuPont Teijin para-aramid chopped PPTA, and nano-aramid fiber in a mass ratio of 1:4:2:1.

[0055] Preparation method of nano-aramid fiber: Preparation of aramid nanofiber (ANF) by proton donor-assisted deprotonation S ) dispersion U51, specifically, 2 g of para-aramid PPTA fiber was weighed and placed in a mixed solution of 3 g KOH, 1.0 L DMSO and 40 mL deionized water, and stirred in a water bath at 60 ° C for 3 h to obtain a dark red ANF with a mass concentration of 2 g / L. S Dispersion, using nanofiltration to obtain aramid nanofibers ANF S pink.

[0056] The flaky filler is composed of molybdenum sulfide nanosheets (brand Yamei Nano, MoS2-200nm molybdenum disulfide nanosheets), boron nitride nanosheets (brand Yamei Nano, hBN-500nm boron nitride nanosheets), and ultrafine mica sheets in a mass ratio of 5:5:90.

[0057] Preparation method of ultrafine mica flakes: Use 60-mesh high thermal conductivity insulation phlogopite from Shijiazhuang Chenjin Mineral Products Co., Ltd. as raw material for high-speed ball milling, use zirconium oxide as grinding beads, and ball mill at a speed of 300rpm for 60 minutes. Sieve with a 1250 sieve, and the sieved material is the ultrafine mica flakes.

[0058] A preparation process of a plastic-steel PPS composite material comprises the following steps: Step 1, first prepare a filler composition, and evenly mix the spherical filler, the fibrous filler, and the flaky filler in a mass ratio of 60:20:20; then perform surface modification treatment on the prepared filler composition: place the filler composition in a surface modification liquid (the surface modification liquid is composed of a surface modifier and deionized water, and 100 parts of the surface modification liquid contain 6 parts of K570 coupling agent and 2 parts of dispersant titanate coupling agent HY-311) for ultrasonic dispersion treatment for 30 minutes, the ultrasonic dispersion frequency is 44kHz, the power is 800W, and the finished filler composition is drained and dried; At the same time, the aramid fiber-based woven fabric is subjected to surface modification process to obtain the finished aramid fiber-based woven fabric: S1.1, the aramid fiber-based woven fabric is ultrasonically cleaned in an ethanol-water solution (the volume of ethanol and deionized water is 1 / 4), the ultrasonic dispersion frequency is 44kHz, the power is 800W, and after completion, it is rinsed with clean water, dried, and set aside; S1.2, treating the aramid fiber-based woven fabric with low-temperature plasma, first with ozone at 0-4°C for 100 seconds, and then with ammonia at 0-4°C for 120 seconds, to obtain a semi-finished aramid fiber-based woven fabric; S1.3, placing the aramid fiber-based woven fabric that has completed the low-temperature plasma treatment in a KH570 aqueous solution (KH570 concentration is 8wt%), heating to 50°C for ultrasonic dispersion treatment for 30 minutes, with an ultrasonic dispersion frequency of 44kHz and a power of 800W. After the ultrasonic dispersion treatment is completed, the aramid fiber-based woven fabric is taken out, drained and dried to obtain a finished aramid fiber-based woven fabric; Step 2, the filler composition in step 1 and the correctly measured PPS resin, hyperbranched PPS resin, K550 coupling agent, K570 coupling agent, titanate coupling agent HY-311, antioxidant 1024, and antioxidant 168 are mixed and dispersed uniformly at high speed, and then put into a twin-screw extruder, and the four temperature sections of the barrel end temperature are set to 300° C., 315° C., 325° C., and 325° C. in sequence, the nozzle temperature is 325° C., the injection pressure is 95 MPa, the injection speed is 45 mm / s, and the screw rotation speed is 54 rpm. The molten extrudate ejected from the nozzle is subjected to wire drawing, nitrogen cooling, granulation, and drying (140° C. / 3 h) to obtain a PPS composite masterbatch; Step 3, putting the prepared PPS composite masterbatch into a twin-screw extruder, setting the four temperature sections of the barrel end temperature to 300°C, 315°C, 325°C, and 325°C in sequence, the nozzle temperature to 325°C, the mold temperature to 145°C, the injection pressure to 100MPa, the injection speed to 60mm / s, the holding pressure to 55MPa, the screw rotation speed to 65rpm, and injection molding to obtain a PPS sheet with a thickness of 0.35mm; Step 4: stack to form a PPS sheet / finished aramid fiber-based woven fabric / PPS sheet structure, hot press at 288°C and 8MPa for 500s to obtain a PPS composite sheet, heat treat the obtained PPS composite sheet at 155°C for 45min, and naturally cool to room temperature to obtain a plastic-steel PPS composite sheet that meets the use requirements of battery shell materials.

[0059] The difference between Example 2 and Example 1 is that the modified PPS matrix resin is made of the following raw materials in parts by mass: 100 parts of PPS resin, 10 parts of hyperbranched PPS resin, 52.4 parts of filler composition, 0.65 parts of dispersant K550 coupling agent, 0.65 parts of dispersant K570 coupling agent, 0.22 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0060] The difference between Example 3 and Example 1 is that the modified PPS matrix resin is made of the following raw materials in parts by mass: 100 parts of PPS resin, 15 parts of hyperbranched PPS resin, 54.7 parts of filler composition, 0.68 parts of dispersant K550 coupling agent, 0.68 parts of dispersant K570 coupling agent, 0.26 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0061] The difference between Example 4 and Example 1 is that the modified PPS matrix resin is made of the following raw materials in parts by mass: 100 parts of PPS resin, 20 parts of hyperbranched PPS resin, 57.1 parts of filler composition, 0.72 parts of dispersant K550 coupling agent, 0.72 parts of dispersant K570 coupling agent, 0.28 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0062] The difference between Example 5 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 15 parts of hyperbranched PPS resin, 60 parts of filler composition, 0.75 parts of dispersant K550 coupling agent, 0.75 parts of dispersant K570 coupling agent, 0.3 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0063] The difference between Example 6 and Example 1 is that the modified PPS matrix resin is made of the following raw materials in parts by mass: 100 parts of PPS resin, 15 parts of hyperbranched PPS resin, 70 parts of filler composition, 0.85 parts of dispersant K550 coupling agent, 0.85 parts of dispersant K570 coupling agent, 0.3 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0064] The difference between Example 7 and Example 3 is that the filler composition is composed of spherical fillers, fibrous fillers and flaky fillers in a mass ratio of 40:30:30.

[0065] The difference between Example 8 and Example 3 is that the filler composition is composed of spherical fillers, fibrous fillers and flaky fillers in a mass ratio of 50:30:20.

[0066] The difference between Example 9 and Example 3 is that the filler composition is composed of spherical fillers, fibrous fillers and flaky fillers in a mass ratio of 60:25:15.

[0067] The difference between Example 10 and Example 3 is that the filler composition is composed of spherical fillers, fibrous fillers and flaky fillers in a mass ratio of 70:20:10.

[0068] The difference between Example 11 and Example 9 is that the filler composition is composed of spherical fillers, fibrous fillers and flaky fillers in a mass ratio of 80:10:10.

[0069] The difference between Example 12 and Example 9 is that the filler composition is composed of spherical fillers, fibrous fillers and flaky fillers in a mass ratio of 90:5:5.

[0070] The difference between Example 13 and Example 9 is that the spherical alumina is composed of nano spherical alumina with an average particle size of 300 nm, ultrafine spherical alumina with an average particle size of 3±1 μm, and spherical alumina with an average particle size of 30±3 μm in a mass ratio of 20:50:30.

[0071] The difference between Example 14 and Example 9 is that the spherical alumina is composed of nano spherical alumina with an average particle size of 300 nm, ultrafine spherical alumina with an average particle size of 3±1 μm, and spherical alumina with an average particle size of 30±3 μm in a mass ratio of 25:35:45.

[0072] The difference between Example 15 and Example 9 is that the spherical alumina is composed of nano spherical alumina with an average particle size of 300 nm, ultrafine spherical alumina with an average particle size of 3±1 μm, and spherical alumina with an average particle size of 30±3 μm in a mass ratio of 10:80:10.

[0073] The difference between Example 16 and Example 9 is that the spherical alumina is composed of nano spherical alumina with an average particle size of 300 nm, ultrafine spherical alumina with an average particle size of 3±1 μm, and spherical alumina with an average particle size of 30±3 μm in a mass ratio of 30:40:30.

[0074] The difference between Example 17 and Example 9 is that the spherical alumina is ultrafine spherical alumina with an average particle size of 0.5-5 μm.

[0075] The difference between Example 18 and Example 9 is that the spherical filler is composed of spherical aluminum oxide, spherical silicon nitride, and spherical titanium nitride in a mass ratio of 85:10:5.

[0076] The difference between Example 19 and Example 9 is that the spherical filler is composed of spherical aluminum oxide, spherical silicon nitride, and spherical titanium nitride in a mass ratio of 90:5:5.

[0077] The difference between Example 20 and Example 9 is that the spherical filler is composed of spherical aluminum oxide, spherical silicon nitride, and spherical titanium nitride in a mass ratio of 95:3:2.

[0078] The difference between Example 21 and Example 9 is that the spherical filler is only spherical alumina. The spherical alumina is composed of nano spherical alumina with an average particle size of 300nm, ultrafine spherical alumina with an average particle size of 3±1 μm, and spherical alumina with an average particle size of 30±3 μm in a mass ratio of 15:60:25. The difference between Example 22 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers in a mass ratio of 65:30:2:3.

[0079] The difference between Example 23 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers in a mass ratio of 60:35:2:3.

[0080] The difference between Example 24 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers in a mass ratio of 55:45:2:3.

[0081] The difference between Example 25 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers in a mass ratio of 45:50:2:3.

[0082] The difference between Example 26 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers in a mass ratio of 35:60:2:3.

[0083] The difference between Example 27 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, and potassium titanate whiskers in a mass ratio of 62:35:3.

[0084] The difference between Example 28 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, and zinc oxide whiskers in a mass ratio of 63:35:2.

[0085] The difference between Example 29 and Example 18 is that the fibrous filler is composed of a chopped aramid fiber composition and single-walled carbon nanotubes in a mass ratio of 65:35.

[0086] The difference between Example 30 and Example 23 is that the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets in a mass ratio of 10:10:80.

[0087] The difference between Example 31 and Example 23 is that the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets in a mass ratio of 15:15:70.

[0088] The difference between Example 32 and Example 23 is that the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets in a mass ratio of 20:20:60.

[0089] The difference between Example 33 and Example 23 is that the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets in a mass ratio of 25:25:50.

[0090] The difference between Example 34 and Example 23 is that the flaky filler is composed of boron nitride nanosheets and ultrafine mica sheets in a mass ratio of 5:95.

[0091] The difference between Example 35 and Example 23 is that the flaky filler is composed of molybdenum sulfide nanosheets and ultrafine mica sheets in a mass ratio of 5:95.

[0092] The difference between Example 36 and Example 23 is that the flaky filler is only ultrafine mica flakes.

[0093] The difference between Example 37 and Example 23 is that the ultrafine mica flakes are replaced by surface carbon nanotube grafted modified mica flakes. That is, the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, and surface carbon nanotube grafted modified mica flakes in a mass ratio of 5:5:90. The preparation method of surface carbon nanotube grafted modified mica flakes (commissioned by Zhejiang Rongtai Technology) is as follows: Step 1: At room temperature, add 0.02 mol of 2-ethyl-4-methylimidazole 2E4MI and 0.01 mol of silver acetate AgAc into 400 mL of dichloromethane, stir magnetically at a speed of 240 r / min until the AgAc particles completely disappear to obtain a clear and transparent Ag(2E4MI)2Ac complex solution; Step 2: Add 0.5 g of CNTs (TNGM2, Chengdu Institute of Organic Chemistry, Chinese Academy of Sciences) and 0.5 g of PVP to the Ag(2E4MI)2Ac complex solution, use ultrasonic dispersion (power 1200 W, frequency 40 kHz) for 3 h, add 50 g of ultrafine mica flakes, and continue ultrasonic dispersion for 0.5 h to obtain a dispersion.

[0094] Step 3: subjecting the dispersion obtained in step 2 to vacuum distillation to remove dichloromethane from the dispersion and subjecting the solid to high-temperature sintering, wherein the high-temperature sintering temperature is controlled at 210° C. and the high-temperature sintering time is 4 hours to obtain a solid; Step 4: The solid obtained in step 3 is placed in a three-roll mill for three times grinding and crushing, the roller spacing of the three-roll mill is 30 μm, and then dispersed in 400 mL of ethanol, poured into a basket grinder for grinding, and ground at a speed of 2000 r / min for 0.5 h, and then filtered and dried to obtain ultrafine mica flakes-CNTs hybrid materials.

[0095] The difference between Example 38 and Example 21 is that the ultrafine mica flakes are replaced by surface graphene grafted modified mica flakes. That is, the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, and surface graphene grafted modified mica flakes in a mass ratio of 5:5:90. The preparation method of surface graphene grafted modified mica flakes (commissioned by Zhejiang Rongtai Technology) is as follows: Step 1: At room temperature, add 0.02 mol of 2-ethyl-4-methylimidazole 2E4MI and 0.01 mol of silver acetate AgAc into 400 mL of dichloromethane, stir magnetically at a speed of 240 r / min until the AgAc particles completely disappear to obtain a clear and transparent Ag(2E4MI)2Ac complex solution; Step 2: Add 0.5 g of graphene nanosheets (industrial-grade nanographene sheets TNIGNP, Chengdu Institute of Organic Chemistry, Chinese Academy of Sciences) and 0.5 g of PVP to the Ag(2E4MI)2Ac complex solution, use ultrasonic dispersion (power 1200 W, frequency 40 kHz) for 3 h, add 50 g of ultrafine mica flakes, and continue ultrasonic dispersion for 0.5 h to obtain a dispersion.

[0096] Step 3: subjecting the dispersion obtained in step 2 to vacuum distillation to remove dichloromethane from the dispersion and subjecting the solid to high-temperature sintering, wherein the high-temperature sintering temperature is controlled at 210° C. and the high-temperature sintering time is 4 hours to obtain a solid; Step 4: The solid obtained in step 3 is placed in a three-roll mill for three times grinding and crushing, the roller spacing of the three-roll mill is 30 μm, and then dispersed in 400 mL of ethanol, poured into a basket grinder for grinding, and ground at a speed of 2000 r / min for 0.5 h, and then filtered and dried to obtain ultrafine mica flakes-CNTs hybrid materials.

[0097] The difference between Example 39 and Example 21 is that the ultrafine mica flakes are replaced by surface graphene grafted modified mica flakes and surface carbon nanotube grafted modified mica flakes. That is, the flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, surface graphene grafted modified mica flakes in Example 33, and surface carbon nanotube grafted modified mica flakes in Example 32 in a mass ratio of 5:5:45:45.

[0098] The difference between Example 40 and Example 1 is that the aramid fiber-based woven fabric is a plain weave warp-weft structure, the warp is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 1mm. The weft is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 1mm, that is, the aramid fiber-based woven fabric is formed with a 1mm*1mm mesh.

[0099] The difference between Example 41 and Example 1 is that the aramid fiber-based woven fabric is a plain weave warp-weft structure, the warp is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 0.5 mm. The weft is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 0.5 mm, that is, the aramid fiber-based woven fabric is formed with a mesh of 0.5 mm*0.5 mm.

[0100] The difference between Example 42 and Example 1 is that the aramid fiber-based woven fabric is a plain weave warp-weft structure, the warp is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 2mm. The weft is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 2mm, that is, the aramid fiber-based woven fabric is formed with a 2mm*2mm mesh.

[0101] The difference between Example 43 and Example 1 is that the aramid fiber-based woven fabric is a plain weave warp-weft structure, the warp is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 3mm. The weft is aramid fiber (Japanese Kuraray Vectran 50D aramid bulletproof yarn) and 1K Toray carbon fiber filaments, and the interval between the aramid fiber and the adjacent carbon fiber filaments is 3mm, that is, the aramid fiber-based woven fabric is formed with a 3mm*3mm mesh.

[0102] The difference between Example 44 and Example 1 is that in step 1, the aramid fiber-based woven fabric is subjected to a surface modification process to obtain a finished aramid fiber-based woven fabric, and the specific surface modification process is as follows: S1.1, the aramid fiber-based woven fabric is ultrasonically cleaned in an ethanol-water solution (the volume of ethanol and deionized water is 1 / 4), the ultrasonic dispersion frequency is 44kHz, the power is 800W, and after completion, it is rinsed with clean water, dried, and set aside; S1.2, firstly subjecting the aramid fiber-based woven fabric to low-temperature plasma treatment, firstly subjecting the aramid fiber-based woven fabric to low-temperature plasma treatment at 0-4°C for 100s, and then subjecting the aramid fiber-based woven fabric to low-temperature plasma treatment at 0-4°C for 120s, to obtain a semi-finished aramid fiber-based woven fabric; then subjecting the aramid fiber-based woven fabric in S1.1 to sol-gel treatment, so that nano-alumina particles are generated in situ on the surface of the warp and weft in the aramid fiber-based woven fabric, thereby realizing surface alumina doping modification of the aramid fiber-based woven fabric; S1.3, place the surface alumina-doped modified aramid fiber-based woven fabric in a KH570 aqueous solution (KH570 concentration is 8wt%), heat it to 50°C and carry out ultrasonic dispersion treatment for 30 minutes, the ultrasonic dispersion frequency is 44kHz, and the power is 800W. After completing the ultrasonic dispersion treatment, take out the aramid fiber-based woven fabric, drain it and dry it to obtain the finished aramid fiber-based woven fabric.

[0103] The difference between Example 45 and Example 44 is that the filler composition is composed of spherical fillers, fibrous fillers, and flaky fillers in a mass ratio of 60:25:15. The spherical filler is composed of spherical aluminum oxide, spherical silicon nitride, and spherical titanium nitride in a mass ratio of 85:10:5. The fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers in a mass ratio of 60:35:2:3. The flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets, the surface graphene grafted modified mica sheets in Example 33, and the surface carbon nanotube grafted modified mica sheets in Example 32 in a mass ratio of 5:5:45:45.

[0104] The difference between Comparative Example 1 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 5 parts of hyperbranched PPS resin, 40 parts of filler composition, 0.45 parts of dispersant K550 coupling agent, 0.45 parts of dispersant K570 coupling agent, 0.12 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0105] The difference between Comparative Example 2 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 5 parts of hyperbranched PPS resin, 80 parts of filler composition, 0.9 parts of dispersant K550 coupling agent, 0.9 parts of dispersant K570 coupling agent, 0.24 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0106] The difference between Comparative Example 3 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 0 parts of hyperbranched PPS resin, 47.6 parts of filler composition, 0.5 parts of dispersant K550 coupling agent, 0.5 parts of dispersant K570 coupling agent, 0.15 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0107] The difference between Comparative Example 4 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 2 parts of hyperbranched PPS resin, 48.6 parts of filler composition, 0.55 parts of dispersant K550 coupling agent, 0.55 parts of dispersant K570 coupling agent, 0.17 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0108] The difference between Comparative Example 5 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 22 parts of hyperbranched PPS resin, 58.2 parts of filler composition, 0.8 parts of dispersant K550 coupling agent, 0.8 parts of dispersant K570 coupling agent, 0.3 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0109] The difference between Comparative Example 6 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 5 parts of hyperbranched PPS resin, 50 parts of filler composition, 1.2 parts of dispersant K550 coupling agent, 0 parts of dispersant K570 coupling agent, 0.2 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0110] The difference between Comparative Example 7 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 5 parts of hyperbranched PPS resin, 50 parts of filler composition, 0 parts of dispersant K550 coupling agent, 1.2 parts of dispersant K570 coupling agent, 0.2 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0111] The difference between Comparative Example 8 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 5 parts of hyperbranched PPS resin, 50 parts of filler composition, 1.4 parts of dispersant K550 coupling agent, 0 parts of dispersant K570 coupling agent, 0 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0112] The difference between Comparative Example 9 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 5 parts of hyperbranched PPS resin, 50 parts of filler composition, 0 parts of dispersant K550 coupling agent, 1.4 parts of dispersant K570 coupling agent, 0 parts of dispersant titanate coupling agent HY-311, 1.6 parts of antioxidant 1024, and 0.4 parts of antioxidant 168.

[0113] The difference between Comparative Example 10 and Example 1 is that the modified PPS matrix resin includes the following raw materials in parts by mass: 100 parts of PPS resin, 5 parts of hyperbranched PPS resin, 50 parts of filler composition, 1.2 parts of dispersant K550 coupling agent, 0 parts of dispersant K570 coupling agent, 0.2 parts of dispersant titanate coupling agent HY-311, and 2 parts of antioxidant 1024.

[0114] The difference between Comparative Example 11 and Example 1 is that 50 parts of the filler composition are replaced by 50 parts of spherical fillers.

[0115] The difference between Comparative Example 12 and Example 1 is that 50 parts of the filler composition are replaced by 50 parts of fibrous filler.

[0116] The difference between Comparative Example 13 and Example 1 is that 50 parts of the filler composition are replaced by 50 parts of the flaky filler.

[0117] The difference between Comparative Example 14 and Example 1 is that the filler composition consists of spherical fillers and fibrous fillers in a mass ratio of 6:4.

[0118] The difference between Comparative Example 15 and Example 1 is that the filler composition consists of spherical fillers and flaky fillers in a mass ratio of 6:4.

[0119] The difference between Comparative Example 16 and Example 1 is that the filler composition consists of fibrous filler and flaky filler in a mass ratio of 1:1.

[0120] The difference between Comparative Example 17 and Example 1 is that no aramid fiber-based woven fabric is provided inside the modified PPS matrix resin.

[0121] The difference between Comparative Example 18 and Example 1 is that the aramid fiber-based woven fabric is not subjected to the surface modification process of step one.

[0122] The difference between Comparative Example 19 and Example 1 is that in step 1, the aramid fiber-based woven fabric is subjected to a surface modification process to obtain a finished aramid fiber-based woven fabric, and the specific surface modification process is as follows: S1.1, the aramid fiber-based woven fabric is ultrasonically cleaned in an ethanol-water solution (the volume of ethanol and deionized water is 1 / 4), the ultrasonic dispersion frequency is 44kHz, the power is 800W, and after completion, it is rinsed with clean water, dried, and set aside; S1.2, treating the aramid fiber-based woven fabric with low-temperature plasma, firstly treating the aramid fiber-based woven fabric with low-temperature plasma at 0-4°C for 100s to obtain a semi-finished aramid fiber-based woven fabric; S1.3, place the semi-finished aramid fiber-based woven fabric in S1.2 in a KH570 aqueous solution (KH570 concentration is 8wt%), heat it to 50°C and perform ultrasonic dispersion treatment for 30 minutes, the ultrasonic dispersion frequency is 44kHz, and the power is 800W. After completing the ultrasonic dispersion treatment, take out the aramid fiber-based woven fabric, drain it and dry it to obtain the finished aramid fiber-based woven fabric.

[0123] The control group is the existing 40wt% GF modified polyphenylene sulfide material.

[0124] Performance test: 1. Tensile properties are measured in accordance with ISO 527-2. 2. Simply supported beam impact strength (unnotched) is measured in accordance with ISO 179. 3. Flexural strength is measured in accordance with ISO 178. 4. Dielectric strength (3mm) is measured in accordance with IEC 60243. 5. Thermal conductivity is measured in accordance with GB / T 10295-2008 Determination of steady-state thermal resistance and related properties of thermal insulation materials - Heat flow meter method.

[0125] Table 1: Test parameters of plastic-steel PPS composite plates in Examples 1-6 and Comparative Examples 1-10

[0126] It can be seen from Examples 1-6, Comparative Examples 1-2 and Table 1 that the addition amount of the filler composition is preferably 50-70 parts.

[0127] Combining Examples 1-6, Comparative Examples 3-5 and Table 1, it can be seen that the addition amount of the hyperbranched PPS resin is preferably 5-20 parts. Too low an addition amount will reduce the overall impact toughness; while too high an addition amount will affect the overall mechanical strength.

[0128] Combining Example 1, Comparative Examples 6-9 and Table 1, it can be seen that the dispersant compounded with KH-550 silane coupling agent, KH-570 silane coupling agent and titanate coupling agent HY-311 can effectively disperse the filler composition and improve the overall physical and chemical properties.

[0129] It can be seen from Example 1, Comparative Example 10 and Table 1 that the use of the combination of antioxidant 1024 and antioxidant 168 can improve the thermal oxidative degradation resistance of the PPS resin, that is, improve the anti-aging performance and ensure the overall physical and chemical properties.

[0130] Combining Examples 1-6, Comparative Examples 1-2 and Table 1, it can be seen that the modified PPS matrix resin formula provided in Example 3 is better, the addition amount of the filler composition is 54.7 parts, and the addition amount of the hyperbranched PPS resin is 15 parts.

[0131] Table 2: Test parameters of plastic-steel PPS composite panels in Examples 3, 7-12 and Comparative Examples 11-16

[0132] From Examples 3, 7-12 and Comparative Examples 11-16 and Table 2, it can be seen that the addition of fibrous filler in the filler composition significantly improves the tensile properties, but excessive addition of fibrous filler will lead to a large decrease in insulation strength. Therefore, the proportion of fibrous filler in the filler composition is preferably 20-30wt%, and the preferred amount of fibrous filler added is 25wt%.

[0133] It can be seen from Examples 3, 7-12 and Comparative Examples 11-16 and Table 2 that the spherical filler, fibrous filler and sheet filler are used in a mass ratio of (50-80): (10-30): (10-20) to form a filler composition, which can ensure that the physical and chemical properties of the prepared plastic-steel PPS composite material meet the requirements of battery shell materials. Preferably, the spherical filler, fibrous filler and sheet filler in the filler composition are used in a mass ratio of 60:25:15 to ensure the mechanical strength, impact toughness and heat dissipation of the prepared plastic-steel PPS composite material.

[0134] Table 3: Test parameters of plastic-steel PPS composite panels in Example 9 and Examples 13-21

[0135] It can be seen from Example 9 and Examples 13-17 and Table 3 that the particle size distribution of spherical alumina in the filler composition has a relatively obvious effect on the mechanical strength, impact toughness and heat dissipation of the prepared plastic-steel PPS composite material. When the spherical alumina system is composed of nano-spherical alumina with an average particle size of 300nm, ultrafine spherical alumina with an average particle size of 3±1μm, and spherical alumina with an average particle size of 30±3μm in a mass ratio of (15-25):(35-60):(25-40), the three comprehensive properties of mechanical strength, impact toughness and heat dissipation of the prepared plastic-steel PPS composite material are relatively good, and the production cost can also be reduced.

[0136] It can be seen from Example 9 and Examples 18-21 and Table 3 that the spherical silicon nitride and spherical titanium nitride contained in the spherical filler have a positive effect on the heat aging resistance of the plastic-steel PPS composite material. When the spherical aluminum oxide, spherical silicon nitride and spherical titanium nitride are composed of spherical fillers in a mass ratio of (80-90): (5-10): (5-10), the comprehensive performance of the prepared plastic-steel PPS composite material is relatively good. Preferably, the mass ratio of spherical aluminum oxide, spherical silicon nitride and spherical titanium nitride is 85:10:5.

[0137] Table 4: Test parameters of plastic-steel PPS composite panels in Example 18 and Examples 22-29

[0138] Combining Example 18 and Examples 22-26 with Table 4, it can be seen that the content of single-walled carbon nanotubes in the fibrous filler is preferably 25-50wt% of the total mass of the fibrous filler, and excessive addition will greatly reduce the safety of insulation and electrical breakdown resistance. When the content of single-walled carbon nanotubes accounts for 35wt% of the total mass of the fibrous filler, the comprehensive performance of the plastic-steel PPS composite material is better.

[0139] It can be seen from Example 18 and Examples 27-29 and Table 4 that the addition of appropriate amounts of zinc oxide whiskers and potassium titanate whiskers can improve the tensile properties, impact toughness, resistance to thermal oxidation degradation, and hot extrusion processing performance of the plastic-steel PPS composite material.

[0140] Table 5: Test parameters of plastic-steel PPS composite panels in Example 23 and Examples 30-39

[0141] It can be seen from Example 23 and Example 30-39 and Table 5 that the addition of molybdenum sulfide nanosheets and boron nitride nanosheets has a positive effect on the tensile properties and impact toughness of the plastic-steel PPS composite material. When the molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets are composed in a mass ratio of (5-20): (5-20): (60-90), the comprehensive performance of the prepared plastic-steel PPS composite material is relatively excellent. Preferably, the molybdenum sulfide nanosheets, boron nitride nanosheets, and ultrafine mica sheets are in a mass ratio of 10:10:80.

[0142] It can be seen from Example 30 and Examples 37-39 and Table 5 that the addition of surface carbon nanotube grafted modified mica sheets and / or surface graphene grafted modified mica sheets can improve the thermal conductivity and tensile properties of the plastic-steel PPS composite material while still maintaining relatively good insulation safety performance.

[0143] Table 6: Test parameters of plastic-steel PPS composite plates in Example 1, Examples 40-45, and Comparative Examples 17-19

[0144] Combining Example 1 with Comparative Examples 17-19 and Table 6, it can be seen that the aramid fiber-based woven fabric needs to be subjected to specific surface treatment to achieve better compatibility with the modified PPS matrix resin, thereby improving the overall tensile properties and impact toughness.

[0145] Combining Example 1 with Example 40 and Table 6, it can be seen that the addition of carbon fiber to the aramid fiber-based woven fabric can further improve the tensile properties and impact toughness of the plastic-steel PPS composite material and also have certain insulation and electrical breakdown resistance, meeting the use requirements of battery casing materials.

[0146] Combining Example 1 with Examples 40-43 and Table 6, it can be seen that the mesh size formed by the warp and weft in the aramid fiber-based woven fabric has a certain influence on the mechanical properties and impact strength of the plastic-steel PPS composite material. The mesh size formed by the warp and weft is preferably controlled to be 0.5 mm*0.5 mm to 2 mm*2 mm, and the mesh size formed by the warp and weft is preferably controlled to be 1 mm*1 mm.

[0147] Combining Example 1 with Example 44 and Table 6, it can be seen that in Example 44, the fiber surface of the aramid fiber-based woven fabric is treated by a sol-gel method to in-situ generate nano-alumina particles to improve the overall insulation and electrical breakdown resistance, and also has good heat dissipation, tensile strength and impact toughness.

[0148] In summary, the composite design of the compound filler composition and hyperbranched PPS resin combined with the built-in aramid fiber-based woven fabric adopted in this application effectively improves the overall mechanical strength, thermal stability, chemical corrosion resistance, electrical properties, wear resistance and flame retardancy of the plastic-steel PPS composite material, and at the same time has excellent impact toughness, meeting the requirements of battery casing materials.

[0149] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A plastic-steel PPS composite material, characterized in that: The invention comprises a modified PPS matrix resin and at least one aramid fiber-based woven fabric compounded inside the modified PPS matrix resin, wherein the aramid fiber-based woven fabric is a warp-weft knitted structure of a plain weave structure, wherein the warp threads of the aramid fiber-based woven fabric at least comprise aramid fibers, and the weft threads at least comprise aramid fibers; The modified PPS matrix resin is made of the following raw materials in parts by mass: 100 parts of PPS resin, 5-20 parts of hyperbranched PPS resin, 50-70 parts of filler composition, 0.5-2 parts of dispersant, and 1-3 parts of anti-aging agent; The dispersant is at least one of stearate, siloxane coupling agent and titanate coupling agent; The anti-aging agent is at least one of antioxidant 1024, antioxidant 4426, antioxidant 300, antioxidant 168, and antioxidant 626; The filler composition comprises a combination of spherical fillers, fibrous fillers and flake fillers. The spherical filler includes at least one of spherical alumina, spherical aluminum nitride, spherical silicon dioxide, spherical silicon nitride, spherical titanium nitride, and spherical silicon carbide; The fibrous filler comprises at least one of nanocarbon fibers, chopped aramid fiber compositions, carbon nanotubes, cellulose nanofibers, and inorganic whiskers; The inorganic whiskers include at least one of zinc oxide whiskers, aluminum oxide whiskers, zirconium oxide whiskers, aluminum nitride whiskers, boron nitride whiskers, silicon dioxide whiskers, silicon nitride whiskers, silicon carbide whiskers, calcium carbonate whiskers, and potassium titanate whiskers; The flaky filler includes at least one of graphene nanosheets, boron nitride nanosheets, MXene phase ceramic nanosheets, ultrafine mica sheets, and molybdenum sulfide nanosheets.

2. The plastic-steel PPS composite material according to claim 1, characterized in that: The mass ratio of the spherical filler, the fibrous filler and the flake filler is (50-80):(10-30):(10-20).

3. The plastic-steel PPS composite material according to claim 2, characterized in that: The spherical filler is spherical alumina, spherical silicon nitride, and spherical titanium nitride in a mass ratio of (80-90):(5-10):(5-10); the spherical alumina is composed of nano-spherical alumina with an average particle size of 100-400nm, spherical silicon nitride with an average particle size of 0.5-5 μm Ultrafine spherical alumina, average particle size 25-50 μm The spherical aluminum oxide is composed of a mass ratio of (15-25): (35-60): (25-40); the average particle size of the spherical silicon nitride is 0.8-5 μm; The average particle size of spherical titanium nitride is 0.02-5 μm .

4. The plastic-steel PPS composite material according to claim 3, characterized in that: The fibrous filler is composed of a chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers; the mass ratio of the chopped aramid fiber composition, single-walled carbon nanotubes, zinc oxide whiskers, and potassium titanate whiskers is (40-73):(25-50):(1-5):(1-5).

5. The plastic-steel PPS composite material according to claim 4, characterized in that: The flaky filler is composed of molybdenum sulfide nanosheets, boron nitride nanosheets and ultrafine mica sheets; the mass ratio of the molybdenum sulfide nanosheets, boron nitride nanosheets and ultrafine mica sheets is (5-20):(5-20):(60-90).

6. The plastic-steel PPS composite material according to claim 5, characterized in that: The ultrafine mica sheet is a surface carbon nanotube grafted modified mica sheet and / or a surface graphene grafted modified mica sheet; the surface carbon nanotube grafted modified mica sheet comprises an ultrafine mica sheet carrier with a particle size of ≤1250 mesh and carbon nanotubes fixed to the ultrafine mica sheet carrier with a particle size of ≤1250 mesh by nano-silver sintering; the surface graphene grafted modified mica sheet comprises an ultrafine mica sheet carrier with a particle size of ≤1250 mesh and graphene nanosheets fixed to the ultrafine mica sheet carrier with a particle size of ≤1250 mesh by nano-silver sintering.

7. The plastic-steel PPS composite material according to claim 5, characterized in that: The mass ratio of the spherical filler, the fibrous filler and the flaky filler is (55-60):(20-25):(15-20); the dispersant is composed of KH-550 silane coupling agent, KH-570 silane coupling agent and titanate coupling agent HY-311 in a mass ratio of (0.5-2):(0.5-2):(0.1-0.4).

8. The plastic-steel PPS composite material according to claim 1, characterized in that: The aramid fiber-based woven fabric is a plain weave structure with a warp-weft knitted structure, wherein the interval between adjacent warps is 0.5-2 mm; the interval between adjacent wefts is 0.5-2 mm; the warps in the aramid fiber-based woven fabric include aramid fiber filaments and carbon fiber filaments arranged at intervals from each other; the wefts in the aramid fiber-based woven fabric include aramid fiber filaments and carbon fiber filaments arranged at intervals from each other.

9. A plastic-steel PPS composite material according to claim 1 or 8, characterized in that: The aramid fiber-based woven fabric needs to be subjected to a surface modification process before use; the surface modification process of the aramid fiber-based woven fabric is as follows: Step 1: the aramid fiber-based woven fabric is ultrasonically cleaned in an ethanol aqueous solution, then rinsed with clean water, dried, and set aside; Step 2, treating the aramid fiber-based woven fabric with low-temperature plasma, first with ozone at 0-4°C for 60-300s, and then with ammonia at 0-4°C for 60-300s, to obtain a semi-finished aramid fiber-based woven fabric; Step three, placing the aramid fiber-based woven fabric that has completed the low-temperature plasma treatment in a methacryloxysilane aqueous solution, heating it to 45-50°C for ultrasonic dispersion treatment for 20-40 minutes, wherein the methacryloxysilane concentration in the methacryloxysilane aqueous solution is 4-8wt%. After completing the ultrasonic dispersion treatment, take out the aramid fiber-based woven fabric, drain it and dry it to obtain the finished aramid fiber-based woven fabric.

10. A process for preparing a plastic-steel PPS composite material according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1, first prepare a filler composition, and then perform surface modification treatment on the prepared filler composition: place the filler composition in a surface modification liquid for ultrasonic dispersion treatment for 20-40 minutes, drain and dry to obtain a finished filler composition; the surface modification liquid is composed of a surface modifier and deionized water, and the surface modifier is a siloxane coupling agent and / or a titanate coupling agent; At the same time, the aramid fiber-based woven fabric is subjected to a surface modification process to obtain a finished aramid fiber-based woven fabric; Step 2, the filler composition in step 1 is mixed and dispersed uniformly with the correctly measured PPS resin, hyperbranched PPS resin, dispersant and anti-aging agent at high speed, and then put into a twin-screw extruder, and melt-extruded, wire-drawn, nitrogen-cooled, granulated and dried at a barrel end temperature of 285-325° C. to obtain a PPS composite masterbatch; Step 3, using PPS composite masterbatch for injection molding to form a PPS sheet with a thickness of 0.25-0.40 mm; Step 4: stacking to form a PPS sheet / finished aramid fiber-based woven fabric / PPS sheet structure, hot pressing at 280-300°C and 5-15MPa for 5-15min to obtain a PPS composite sheet, heat treating the obtained PPS composite sheet at 140-160°C for 30-60min, and naturally cooling to room temperature to obtain a plastic-steel PPS composite sheet that meets the use requirements of battery shell materials.

Citation Information

Patent Citations

  • Modified polyphenylene sulfide and preparation method thereof

    CN101125924A

  • Aramid fiber modified polyphenylene sulfide composite material, and preparation method and application thereof

    CN111040207A

  • Lightweight snakelike heat dissipation device for thermal runaway protection of automobile battery cell and preparation method of lightweight snakelike heat dissipation device

    CN117965026A

Cited By

  • A kind of ultra-high voltage mica paper and its preparation process

    CN119777210A

  • High-temperature-resistant PPS cable sheath and preparation method thereof

    CN120464199A

  • Wood household spontaneous heating plate structure with efficient heat dissipation function and preparation method of wood household spontaneous heating plate structure

    CN120481011A