Environment-friendly BOPP film and preparation method thereof

By using the core layer of PP new material, PCR recycled material and antioxidant in the environmentally friendly BOPP film, as well as the surface layer of PP new material and anti-adhesive agent in the film, combined with specific process conditions, the fish eye/crystal point defects and crystal point defects in the film are solved and Due to insufficient mechanical properties, environmentally friendly BOPP film preparation with high quality and excellent mechanical properties has been achieved.

CN119058200APending Publication Date: 2024-12-03GUANGDONG HUATONG NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411350548.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

After adding more than 30% of PCR recycled materials in the existing environmentally friendly BOPP film, fisheye/crystal point defects are prone to appear on the membrane surface and insufficient mechanical properties.

Method used

The core layer consists of PP new material, PCR recycled material and antioxidant, as well as the surface layer one and two composed of PP new material and anti-adhesive agent, is melt-plasticized, filtered, and co-extruded through a twin screw extruder. The melting sheet cooling molding, longitudinal and transverse stretching are prepared, and the density and melt index of PCR recycled materials are controlled to ensure the quality and mechanical properties of the film.

Benefits of technology

The number of fisheyes/crystal points on the film surface is effectively controlled, the mechanical properties of the film is improved, the appearance quality and application performance of the product are ensured, and the tensile strength and elongation of break are excellent.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of BOPP film preparation, and particularly discloses an environment-friendly BOPP film. The environment-friendly BOPP film comprises a surface layer I, a core layer and a surface layer II, the core layer comprises a PP (polypropylene) new material, a PCR (polymerase chain reaction) regenerated material and an antioxidant; the surface layer I and the surface layer II comprise a PP new material and an anti-sticking agent; wherein the mass ratio of the PCR reworked material in the core layer is 35-85%; the core layer comprises the following components in percentage by mass: 35-85% of a PCR reworked material; 1-3% of an antioxidant; the balance is a PP new material. The environment-friendly BOPP film prepared by adding more than 30% of the PCR reworked material not only solves the problem of many flaws such as fish eyes / crystal points on the film surface, but also has better mechanical properties; wide application prospects are realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of BOPP film preparation, in particular to an environmentally friendly BOPP film. Background Art

[0002] With the continuous improvement of global environmental awareness, environmentally friendly packaging materials have become the development trend of the packaging industry. As an important packaging material, GRS-PCR recycled environmentally friendly BOPP film is widely used in many industries such as food, medicine, and cosmetics.

[0003] The environmentally friendly BOPP film is a BOPP film prepared by adding PCR recycled materials; the inventors found in actual production that when the environmentally friendly BOPP film is prepared by adding more than 30% PCR recycled materials, fisheyes / crystal points of varying sizes will be produced on the film surface, and its mechanical properties need to be further improved. Summary of the invention

[0004] In order to overcome at least one of the technical problems existing in the prior art, the present invention provides an environmentally friendly BOPP film.

[0005] The technical solution of the present invention is as follows:

[0006] The present invention first provides an environmentally friendly BOPP film, which comprises a first surface layer, a core layer and a second surface layer;

[0007] The core layer comprises PP new material, PCR recycled material and antioxidant;

[0008] Layer 1 and

[0009] The second surface layer contains PP new material and anti-sticking agent;

[0010] Among them, the mass proportion of PCR recycled materials in the core layer is 35-85%.

[0011] Preferably, the core layer contains the following components in percentage by mass:

[0012] PCR recycled material 35-85%; antioxidant 1-3%; the rest is PP new material.

[0013] Preferably, the surface layer 1 and the surface layer 2 contain the following components in mass percentage:

[0014] Anti-adhesive agent 1-3%; the rest is PP new material.

[0015] Preferably, the PCR regenerated material in the core layer has a density of 0.9 g / cm 3 ~0.92g / cm 3 PCR

[0016] Recycled material.

[0017] Preferably, the PCR regenerated material in the core layer uses a PCR regenerated material with a melt index of 6.0 to 20 g / 10 min. 230°C.

[0018] The inventors found in their research that in the production of environmentally friendly BOPP film, the film prepared from PCR recycled materials with the above-mentioned density, molding shrinkage rate and melt index can effectively control the number of defects such as fish eyes / crystal points on the film surface while ensuring smooth production and good quality, and eliminate the influence of impurities in PCR recycled materials on the product appearance quality.

[0019] Preferably, the thickness of the first surface layer is 1.0 to 1.2 μm; the thickness of the core layer is 18 to 58 μm; the thickness of the second surface layer is 1.0 to 1.2 μm;

[0020] The present invention also provides a method for preparing the above-mentioned environmentally friendly BOPP film, which comprises the following steps:

[0021] (1) Mix the raw materials of each layer according to weight percentage;

[0022] (2) Melting and plasticizing in an extruder;

[0023] (3) The filter screen filters out impurities;

[0024] (4) Three-layer coextrusion;

[0025] (5) The melt is cooled and formed;

[0026] (6) performing longitudinal stretching and transverse stretching;

[0027] (7) After further winding, the environmentally friendly BOPP film is obtained.

[0028] Preferably, the specific conditions for melt plasticization in step (2) are: melt extrusion is performed using a twin-screw extruder, and the temperature of the extruder is controlled at 200-240°C.

[0029] Studies have shown that at this temperature, PP new materials and PCR recycled materials can be fully melted and plasticized, while ensuring that the PCR recycled material is fully melted and plasticized without yellowing or coking.

[0030] Preferably, the specific conditions for cooling and molding the molten sheet in step (5) are: water cooling at 30-35°C.

[0031] Preferably, the specific conditions for longitudinal stretching and transverse stretching in step (6) are:

[0032] The specific conditions for longitudinal stretching are: preheating temperature 135-145°C, stretching ratio 4.8-5.0 times.

[0033] Preferably, the specific conditions for longitudinal stretching and transverse stretching in step (6) are:

[0034] Specific conditions for transverse stretching: preheating temperature 170-175°C, stretching multiple 8-8.5 times.

[0035] The inventors found in further research that in the preparation process of the film of the present invention, the selection of specific conditions of melt plasticization, melt cooling and forming, longitudinal stretching and transverse stretching also plays an important role in the mechanical properties of the prepared film; the study shows that the environmentally friendly BOPP film material prepared under the above-mentioned conditions of melt plasticization, melt cooling and forming, longitudinal stretching and transverse stretching of the present invention has good mechanical properties.

[0036] Preferably, the surface layer of the environmentally friendly BOPP film of the present invention is further subjected to corona treatment.

[0037] Beneficial effects: The present invention provides a new environmentally friendly BOPP film and a preparation method thereof; studies have shown that the environmentally friendly BOPP film prepared by adding more than 30% of PCR recycled materials in the present invention not only has no defects such as fish eyes / crystal points on the film surface, but also has good mechanical properties; it has broad application prospects.

[0038] Specifically referring to GB / T 1040.3, the environmentally friendly BOPP film prepared by the present invention has a tensile strength (MD) of 115 to 135 N / mm 2 , tensile strength (TD) is 250~270N / mm 2 ; Its elongation at break (MD) is 160-190%, and its elongation at break (TD) is 50-65%; It has excellent mechanical properties. In addition, referring to GB / T 2410 standard, the haze of the environmentally friendly BOPP film prepared by the present invention is 2.0-4.0%; referring to GB / T8807 standard, the glossiness of the environmentally friendly BOPP film prepared by the present invention at 45° is 85-90%. DETAILED DESCRIPTION

[0039] The present invention is further explained below in conjunction with specific examples, but the examples do not limit the present invention in any form.

[0040] Example 1 Preparation of environmentally friendly BOPP film

[0041] The environmentally friendly BOPP film is composed of a surface layer 1, a core layer and a surface layer 2; the thickness of the surface layer 1 is 1 μm; the thickness of the core layer is 58 μm; the thickness of the surface layer 2 is 1 μm;

[0042] The core layer is made of the following components by mass percentage: 35% PCR recycled material;

[0043] Oxidation

[0044] Agent 1%; the rest is PP new material;

[0045] The surface layer 1 and the surface layer 2 are respectively made of the following components in percentage by mass: 1% anti-adhesive agent; the remainder is PP new material;

[0046] Among them, the PCR recycled material in the core layer adopts a density of 0.9g / cm 3 , shrinkage rate, melt index of 6.0g / 10min.230℃ PCR recycled material;

[0047] Preparation method:

[0048] (1) Mix the raw materials of each layer according to weight percentage;

[0049] (2) Melting and plasticizing in an extruder;

[0050] (3) The filter screen filters out impurities;

[0051] (4) Three-layer coextrusion;

[0052] (5) The melt is cooled and formed;

[0053] (6) performing longitudinal stretching and transverse stretching;

[0054] (7) After further winding, the environmentally friendly BOPP film is obtained.

[0055] The specific conditions of melt plasticization in step (2) are: melt extrusion using a twin-screw extruder, and the temperature of the extruder is controlled at 200°C.

[0056] The specific conditions for cooling and molding the molten sheet in step (5) are: water cooling at 30°C.

[0057] The specific conditions for longitudinal stretching and transverse stretching in step (6) are as follows: the specific conditions for longitudinal stretching are as follows: preheating temperature 135° C., stretching ratio 4.8 times.

[0058] The specific conditions for the longitudinal stretching and the transverse stretching in step (6) are as follows: The specific conditions for the transverse stretching are: preheating temperature 170° C., and stretching ratio 8 times.

[0059] Example 2 Preparation of environmentally friendly BOPP film

[0060] The environmentally friendly BOPP film is composed of a surface layer 1, a core layer and a surface layer 2; the thickness of the surface layer 1 is 1.2 μm; the thickness of the core layer is 18 μm; the thickness of the surface layer 2 is 1.2 μm;

[0061] The core layer is made of the following components by mass percentage: 85% PCR recycled material;

[0062] Oxidation

[0063] Agent 3%; the rest is PP new material;

[0064] The surface layer 1 and the surface layer 2 are respectively made of the following components in percentage by weight: 3% anti-adhesive agent; the remainder is PP new material;

[0065] Among them, the PCR recycled material in the core layer adopts a density of 0.92g / cm 3 , shrinkage rate, melt index of 20g / 10min. PCR recycled material at 230℃;

[0066] Preparation method:

[0067] (1) Mix the raw materials of each layer according to weight percentage;

[0068] (2) Melting and plasticizing in an extruder;

[0069] (3) The filter screen filters out impurities;

[0070] (4) Three-layer coextrusion;

[0071] (5) The melt is cooled and formed;

[0072] (6) performing longitudinal stretching and transverse stretching;

[0073] (7) After further winding, the environmentally friendly BOPP film is obtained.

[0074] The specific conditions for melt plasticization in step (2) are: melt extrusion using a twin-screw extruder, and the extruder temperature is controlled at 240°C.

[0075] The specific conditions for cooling and molding the molten sheet in step (5) are: water cooling at 35°C.

[0076] The specific conditions for longitudinal stretching and transverse stretching in step (6) are as follows: the specific conditions for longitudinal stretching are as follows: preheating temperature 145° C., stretching ratio 5 times.

[0077] The specific conditions for the longitudinal stretching and the transverse stretching in step (6) are as follows: The specific conditions for the transverse stretching are: preheating temperature 175° C., and stretching ratio 8.5 times.

[0078] Example 3 Preparation of environmentally friendly BOPP film

[0079] The environmentally friendly BOPP film is composed of a surface layer 1, a core layer and a surface layer 2; the thickness of the surface layer 1 is 1 μm; the thickness of the core layer is 40 μm; the thickness of the surface layer 2 is 1 μm;

[0080] The core layer is made of the following components by mass percentage: 50% PCR recycled material;

[0081] Oxidation

[0082] Agent 2%; the rest is PP new material;

[0083] The first and second surface layers are respectively made of the following components in percentage by mass: 2% anti-adhesive agent; the remainder is PP new material;

[0084] Among them, the PCR recycled material in the core layer adopts a density of 0.91g / cm 3 , shrinkage rate, melt index of 10g / 10min.230℃ PCR recycled material;

[0085] Preparation method:

[0086] (1) Mix the raw materials of each layer according to weight percentage;

[0087] (2) Melting and plasticizing in an extruder;

[0088] (3) The filter screen filters out impurities;

[0089] (4) Three-layer coextrusion;

[0090] (5) The melt is cooled and formed;

[0091] (6) performing longitudinal stretching and transverse stretching;

[0092] (7) After further winding, the environmentally friendly BOPP film is obtained.

[0093] The specific conditions for melt plasticization in step (2) are: melt extrusion using a twin-screw extruder, and the extruder temperature is controlled at 220°C.

[0094] The specific conditions for cooling and molding the melt in step (5) are: water cooling at 33°C.

[0095] The specific conditions for longitudinal stretching and transverse stretching in step (6) are as follows: the specific conditions for longitudinal stretching are as follows: preheating temperature 140° C., stretching ratio 4.9 times.

[0096] The specific conditions for the longitudinal stretching and the transverse stretching in step (6) are as follows: The specific conditions for the transverse stretching are: preheating temperature 170° C., and stretching ratio 8.5 times.

Claims

1. An environmentally friendly BOPP film, characterized in that: It includes a surface layer 1, a core layer and a surface layer 2; The core layer comprises PP new material, PCR recycled material and antioxidant; the surface layer and The second surface layer contains PP new material and anti-sticking agent; Among them, the mass proportion of PCR recycled materials in the core layer is 35-85%.

2. The environmentally friendly BOPP film according to claim 1, characterized in that: The core layer contains the following components in percentage by mass: PCR recycled material 35-85%; antioxidant 1-3%; the rest is PP new material. The environmentally friendly BOPP film according to claim 1 is characterized in that the surface layer 1 and the surface layer 2 Layer 2 contains the following components in mass percentage: Anti-adhesive agent 1-3%; the rest is PP new material.

3. The environmentally friendly BOPP film according to claim 1, characterized in that: The PCR recycled material in the core layer has a density of 0.9g / cm 3 ~0.92g / cm 3 PCR recycled material.

4. The environmentally friendly BOPP film according to claim 1, characterized in that: The PCR recycled material in the core layer adopts the PCR recycled material with a melting index of 6.0-20g / 10min.230℃.

5. The environmentally friendly BOPP film according to claim 1, characterized in that: The thickness of the surface layer 1 is 1.0 to 1.2 μm; the thickness of the core layer is 18 to 58 μm; and the thickness of the surface layer 2 is 1.0 to 1.2 μm.

6. The method for preparing the environmentally friendly BOPP film according to any one of claims 1 to 5, characterized in that: The following steps are included: (1) Mix the raw materials of each layer according to weight percentage; (2) Melting and plasticizing in an extruder; (3) The filter screen filters out impurities; (4) Three-layer coextrusion; (5) The melt is cooled and formed; (6) performing longitudinal stretching and transverse stretching; (7) After further winding, the environmentally friendly BOPP film material is obtained.

7. The method for preparing the environmentally friendly BOPP film according to claim 6, characterized in that: The specific conditions of melt plasticization in step (2) are: melt extrusion is carried out using a twin-screw extruder, and the temperature of the extruder is controlled at 200-240°C.

8. The method for preparing the environmentally friendly BOPP film according to claim 6, characterized in that: The specific conditions for cooling and molding the molten sheet in step (5) are: water cooling at 30-35°C.

9. The method for preparing the environmentally friendly BOPP film according to claim 6, characterized in that: The specific conditions for longitudinal stretching and transverse stretching in step (6) are: The specific conditions for longitudinal stretching are: preheating temperature 135-145°C, stretching ratio 4.8-5.0 times.

10. The method for preparing the environmentally friendly BOPP film according to claim 6, characterized in that: The specific conditions for longitudinal stretching and transverse stretching in step (6) are: Specific conditions for transverse stretching: preheating temperature 170-175°C, stretching multiple 8-8.5 times.

Citation Information

Patent Citations

  • Multilayer stretch film comprising PCR plastic waste material

    EP3838587A1

  • Sustainable multilayer film

    US20240246323A1