Sulfide solid electrolyte and preparation method and application thereof

Through the low hardness and low particle size sulfide solid electrolyte, the problem of poor density of the electrolyte layer is solved, the battery performance is improved, and energy consumption is reduced, and more efficient lithium ion transmission is achieved.

CN119059498APending Publication Date: 2024-12-03GTC-POWER ZHUHAI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411299979.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

In high-performance sulfide all-solid state batteries, the electrolyte layer has poor density, resulting in low transmission efficiency of lithium ions and unstable solid contact between electrolyte particles, affecting battery life.

Method used

Using low hardness and low particle size sulfide solid electrolyte, by sintering Li2S, P2S5, LiCl and other raw materials in step by step, combined with rotary sintering and sintering aid, sulfide solid electrolyte with particle size D90≤2μm and hardness less than 120 HB is prepared .

Benefits of technology

It improves the density of the electrolyte membrane, improves the solid interface, improves the battery performance, and reduces the sintering temperature and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059498A_ABST
    Figure CN119059498A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of sulfide solid electrolyte, which comprises the following steps: uniformly mixing Li2S, P2S5 and LiCl to obtain a first mixture; carrying out primary sintering on the first mixture, and cooling to obtain an intermediate sinter; mixing the intermediate sinter with a sintering aid to obtain a second mixture; the second mixture is subjected to secondary sintering, the sulfide solid electrolyte is obtained after cooling, the granularity D90 of primary particles of the sulfide solid electrolyte is smaller than or equal to 2 micrometers, and the hardness of the sulfide solid electrolyte is lower than 120 HB. The invention also provides a sulfide solid electrolyte and a battery. The sulfide solid electrolyte prepared by the preparation method provided by the invention has low hardness and low granularity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to a sulfide solid electrolyte and a preparation method and application thereof. Background Art

[0002] Sulfide all-solid-state batteries have attracted much attention due to their high safety and high energy density, but high-performance sulfide all-solid-state batteries are difficult to build. Among them, affected by the density of the electrolyte layer, the solid-solid contact between the electrolyte particles in the electrolyte layer is unstable, which affects the transmission efficiency of lithium ions. The electrolyte layer expands in volume during the battery cycle, and the density further decreases. The solid-solid contact between the electrolyte particles is further deteriorated, which ultimately affects the battery life.

[0003] The density of the electrolyte is determined by the properties of the electrolyte material and the preparation process, among which the particle size distribution and hardness of the electrolyte material are the main factors: the particle size distribution of the electrolyte material can affect the geometric relationship between the stacking of particles, and the appropriate size distribution can effectively reduce the gaps between particles; and when the particle size distribution is reasonable, the hardness of the material itself will determine the density of the electrolyte layer under the same process. Low-hardness sulfide solid electrolyte materials have higher ductility and can effectively reduce the gaps between materials under the same pressure conditions, thereby improving the density of the electrolyte membrane.

[0004] Therefore, it is necessary to develop a sulfide solid electrolyte with low hardness and low particle size to improve the density of the electrolyte membrane. Summary of the invention

[0005] The purpose of the present application is to provide a sulfide solid electrolyte with low hardness and low particle size to improve the density of the electrolyte membrane.

[0006] In a first aspect, the present application provides a method for preparing a sulfide solid electrolyte, comprising: uniformly mixing Li2S, P2S5, and LiCl to obtain a first mixture; sintering the first mixture once, and obtaining an intermediate sintered product after cooling; mixing the intermediate sintered product with a sintering aid to obtain a second mixture; and sintering the second mixture twice, and obtaining the sulfide solid electrolyte after cooling, wherein the particle size D90 of the primary particles of the sulfide electrolyte is ≤2μm, and the hardness of the sulfide solid electrolyte is lower than 120 HB.

[0007] In some embodiments, the primary sintering temperature is 150-280° C.; the primary sintering time is 2-10 hours.

[0008] In some embodiments, the secondary sintering temperature is 300-400° C.; the secondary sintering time is 2-10 hours.

[0009] In some embodiments, the secondary sintering is rotary sintering; the linear speed of the rotary sintering is 0.5-5 m / min.

[0010] In some embodiments, the sintering aid includes at least one of Li2S, Li2O, P2O5, P2S5, BaO, CaO, MgO, TiO2, SiO2, Al2O3, ZnO, and Y2O3.

[0011] In some embodiments, the sintering aid is 0.2%-1.0wt% of the intermediate sinter by weight.

[0012] In some embodiments, mixing the intermediate sintered material with a sintering aid comprises: crushing the intermediate sintered material; and mixing the crushed intermediate sintered material with the sintering aid.

[0013] In a second aspect, the present application provides a sulfide solid electrolyte, wherein the particle size D90 of primary particles of the sulfide solid electrolyte is ≤2 μm, and the hardness of the sulfide solid electrolyte is less than 120 HB; in powder X-ray diffraction using CuKα rays, the sulfide solid electrolyte has diffraction peaks at 2θ=25.2±0.5deg and 29.7±0.5deg.

[0014] In a third aspect, the present application further provides a battery, comprising the sulfide solid electrolyte as described in the first aspect of the present application or the sulfide solid electrolyte as described in the second aspect of the present application.

[0015] The beneficial effects of the sulfide solid electrolyte and the preparation method thereof provided in this application include but are not limited to the following: 1) The sulfide solid electrolyte provided in the present application has a primary particle size D90≤2μm and a hardness lower than 120HB. The low-hardness sulfide solid electrolyte is used to prepare a highly densified sulfide solid electrolyte layer and improve the solid-solid interface, thereby improving battery performance.

[0016] 2) This application performs step-by-step sintering on the raw materials of the sulfide solid electrolyte, so that the raw materials can nucleate at a lower temperature, reducing the particle size of the primary particles, which is beneficial to reducing the hardness of the electrolyte, and the lower sintering temperature is also beneficial to reducing energy consumption.

[0017] 3) The secondary sintering of the present application is rotary sintering. The dynamic process of rotary sintering can effectively inhibit the agglomeration of primary particles of the material and reduce the particle size of secondary particles, thereby obtaining a sulfide solid electrolyte with small particle size and low hardness. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The following drawings describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only used for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the inventive intent in this application. It should be understood that the drawings are not drawn to scale. Among them: Figure 1 The present invention is a flow chart of a method for preparing a sulfide solid electrolyte according to some embodiments of the present application. DETAILED DESCRIPTION

[0019] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content in the present application. It will be apparent to those skilled in the art that various local modifications to the disclosed embodiments are apparent, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present application. Therefore, the present application is not limited to the embodiments shown, but to the widest scope consistent with the claims.

[0020] The present application provides a preparation method of a sulfide solid electrolyte, comprising: uniformly mixing Li2S, P2S5, and LiCl to obtain a first mixture; sintering the first mixture once, and obtaining an intermediate sintered product after cooling; mixing the intermediate sintered product with a sintering aid to obtain a second mixture; and sintering the second mixture twice, and obtaining the sulfide solid electrolyte after cooling.

[0021] The present application performs step-by-step sintering on the raw materials of the sulfide solid electrolyte so that the raw materials can nucleate at a relatively low temperature. This method is conducive to reducing the hardness of the electrolyte. The particle size D90 of the primary particles of the sulfide electrolyte is ≤2 μm, and the hardness of the sulfide solid electrolyte is lower than 120 HB. In addition, a lower sintering temperature is also conducive to reducing energy consumption. It should be noted that the primary particles described in the present application are particles of single fine grains, also known as the original particle size, and the concept corresponding to the primary particles is secondary particles, that is, secondary particles formed after the primary particles are agglomerated.

[0022] The sulfide solid electrolyte and the preparation method thereof provided in the present application will be described in detail below in conjunction with specific embodiments and drawings.

[0023] refer to Figure 1 , the present application provides a method for preparing a sulfide solid electrolyte, comprising: S1: Mix Li2S, P2S5 and LiCl evenly to obtain a first mixture; S2: sintering the first mixture once, and obtaining an intermediate sintered product after cooling; S3: mixing the intermediate sintered product with a sintering aid to obtain a second mixture; S4: performing secondary sintering on the second mixture, and obtaining the sulfide solid electrolyte after cooling.

[0024] In some embodiments, the Li2S, P2S5, and LiCl are common raw materials for preparing argyrodite-type sulfide solid electrolytes. In some embodiments, the molar ratio of Li2S, P2S5, and LiCl is 2.5:0.5:1, and the sulfide solid electrolyte Li6PS5Cl is prepared.

[0025] In some embodiments, the method of uniformly mixing Li2S, P2S5, and LiCl is high-speed mixing, such as ball milling, crushing, and kneading. High-speed mixing can reduce the particle size of the raw materials and increase the uniformity of mixing.

[0026] In some embodiments, the primary sintering temperature is 150-280°C, for example, 150°C, 160°C, 200°C, 230°C, 250°C or 280°C; the primary sintering time is 2-10 h, for example, 2 h, 3 h, 5 h, 8 h or 10 h.

[0027] In some embodiments, the primary sintering is muffle furnace fixed sintering.

[0028] In some embodiments, mixing the intermediate sintered material with the sintering aid comprises: crushing the intermediate sintered material; and mixing the crushed intermediate sintered material with the sintering aid. By crushing the intermediate sintered material to reduce the particle size of the intermediate sintered material, the intermediate sintered material and the sintering aid can be mixed more uniformly.

[0029] The sintering aid has the functions of lowering the sintering temperature, increasing the density, lowering the thermal expansion coefficient, and improving the mechanical properties.

[0030] In some embodiments, the sintering aid includes at least one of Li2S, Li2O, P2O5, P2S5, BaO, CaO, MgO, TiO2, SiO2, Al2O3, ZnO, and Y2O3.

[0031] In some embodiments, the sintering aid is 0.2%-1.0wt% of the intermediate sinter by weight.

[0032] In some embodiments, the secondary sintering temperature is 300-400°C, for example, 300°C, 320°C, 340°C, 360°C, 380°C or 400°C; the secondary sintering time is 2-10 h, for example, 2 h, 3 h, 5 h, 8 h or 10 h.

[0033] In some embodiments, the secondary sintering is rotary sintering. The dynamic process of rotary sintering can effectively inhibit agglomeration between material particles, which is conducive to obtaining a sulfide solid electrolyte with small particle size and low hardness.

[0034] In some embodiments, the linear speed of the rotational sintering is 0.5-5 m / min, for example, 0.5 m / min, 1 m / min, 1.5 m / min, 3 m / min, 3.5 m / min, 4.5 m / min or 5 m / min.

[0035] Usually, the preparation of sulfide solid electrolyte is carried out by mixing raw materials and sintering them once. The sintering temperature is usually above 450°C, so that the nucleation temperature of the raw materials is high and the crystal nucleus growth rate is fast, so that the particle size of the primary particles of the sulfide solid electrolyte is larger, thereby increasing the hardness of the sulfide solid electrolyte.

[0036] The present application performs step-by-step sintering on the raw materials of the sulfide solid electrolyte, so that the precursor of the sulfide solid electrolyte can form nuclei at a relatively low temperature, and the nuclei grow slowly, which can effectively reduce the particle size of the sulfide solid electrolyte and thus reduce the hardness of the electrolyte. In addition, a lower sintering temperature is also conducive to reducing energy consumption. The particle size D90 of primary particles of the sulfide solid electrolyte is ≤2 μm, and the hardness of the sulfide solid electrolyte is lower than 120 HB.

[0037] In some embodiments, in powder X-ray diffraction using CuKα rays, the sulfide solid electrolyte has diffraction peaks at 2θ=25.2±0.5 deg and 29.7±0.5 deg. Example

[0038] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 h. After the material was cooled, it was crushed and 0.5 wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C, a holding time of 8 h, and a sintering line speed of 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained.

[0039] Li2S, P2S5, and LiCl were weighed in a molar ratio of 2.5:0.5:1, mixed by high-speed mixing, heat treated at 350°C and kept warm for 8 h, and a sulfide solid electrolyte was obtained after the material was cooled.

[0040] Li2S, P2S5, and LiCl were weighed in a molar ratio of 2.5:0.5:1, mixed by high-speed mixing, heat treated at 450°C and kept warm for 8 h, and a sulfide solid electrolyte was obtained after the material was cooled.

[0041] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 h. After the material was cooled, it was crushed and sintered twice at 350°C for 8 h. The sintering line speed was 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained.

[0042] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 h. After the material was cooled, it was crushed and 0.5 wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C and a holding time of 8 h (non-rotating sintering). After the material was cooled, a sulfide solid electrolyte was obtained. Example

[0043] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 150°C and kept warm for 5 h. After the material was cooled, it was crushed and 0.5 wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C, a holding time of 8 h, and a sintering line speed of 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained. Example

[0044] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 8 h. After the material was cooled, it was crushed and 0.5 wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C, a holding time of 8 h, and a sintering line speed of 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained. Example

[0045] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 h. After the material was cooled, it was crushed and 0.2 wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C, a holding time of 8 h, and a sintering line speed of 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained. Example

[0046] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 h. After the material was cooled, it was crushed and 0.5 wt% MgO was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C, a holding time of 8 h, and a sintering line speed of 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained. Example

[0047] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 hours. After the material was cooled, it was crushed and 0.5 wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a secondary sintering temperature of 380°C, a holding time of 8 hours, and a sintering line speed of 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained. Example

[0048] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 hours. After the material was cooled, it was crushed and 0.5wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C, a holding time of 10 hours, and a sintering line speed of 1 m / min. After the material was cooled, a sulfide solid electrolyte was obtained. Example

[0049] Li2S, P2S5 and LiCl were weighed in a molar ratio of 2.5:0.5:1, and the raw materials were mixed by high-speed mixing to obtain an electrolyte precursor. The raw materials were heat treated at 250°C and kept warm for 5 hours. After the material was cooled, it was crushed and 0.5wt% Al2O3 was added. After high-speed mixing, secondary sintering was performed at a temperature of 350°C, a holding time of 8 hours, and a sintering line speed of 2 m / min. After the material was cooled, a sulfide solid electrolyte was obtained. The prepared electrolyte was characterized, including the ionic conductivity, hardness of the material and the porosity of the electrolyte after film preparation. The relevant test methods are as follows: Ionic conductivity test Each sample was pressed into a sheet-like sulfide solid electrolyte material with a diameter of 10 mm and a thickness of 1 mm under the conditions of a water content of less than 10 ppm and a pressure of 200 MPa. Then, an electrochemical impedance spectroscopy (EIS) test was performed at room temperature of 25°C with carbon as the blocking electrode to calculate the ionic conductivity. Hardness test Each sample was prepared into a flaky sulfide solid electrolyte material with a diameter of 10 mm and a thickness of 3 mm under the conditions of a water content of less than 10 ppm and a pressure of 50 MPa, and tested using a digital display Brinell hardness tester. Density test Each sample was prepared into a flaky sulfide solid electrolyte material with a diameter of 20 mm and a thickness of 1 mm under the conditions of a content of less than 10 ppm and a pressure of 500 MPa, and the density was tested by liquid immersion method. Primary particle size test Take an appropriate amount of sulfide solid electrolyte powder, and use a scanning electron microscope (SEM) to observe and count the particle size D90 of the primary particles corresponding to when the cumulative distribution in the sulfide solid electrolyte system reaches 90%. All-solid-state battery assembly and testing The assembly method of the all-solid-state battery is as follows: the positive electrode is the positive electrode plate in the embodiment or the comparative example, the electrolyte layer is Li6PS5Cl, that is, the sulfide solid electrolyte prepared in Examples 1 to 8 and Comparative Examples 1 to 4 of the present application, the electrolyte layer thickness is 30 μm, and the negative electrode is a carbon nano-coated negative electrode.

[0050] The cycle test method is as follows: the charge and discharge voltage is 3.0-4.25V, the cycle temperature is 60°C, the first cycle is 0.05C, and the second cycle starts at 0.3C for 2000 charge and discharge cycles. The indicators for evaluating the cyclability are the first cycle discharge capacity and the capacity retention rate after 500 cycles.

[0051] The results of the above tests are shown in Table 1. Table 1 Performance test results of Examples 1 to 8 and Comparative Examples 1 to 4 From the test data in Table 1, it can be seen that the sulfide solid electrolytes prepared by the preparation method of the present application in Examples 1 to 8 adopt distributed sintering, and rotary sintering and adding a sintering aid during the secondary sintering reduce the particle size and hardness of the sulfide solid electrolyte, and have good electrochemical properties.

[0052] In Comparative Example 1, only one sintering process was used to prepare the sulfide solid electrolyte, and the sintering temperature was low, so that the mixture did not completely form Li6PS5Cl, which reduced the content of the effective ingredients that actually played a role in the sulfide solid electrolyte and affected the electrochemical properties of the sulfide solid electrolyte.

[0053] In Comparative Example 2, only one sintering process is used to prepare the sulfide solid electrolyte. The high sintering temperature results in large primary particle size of the sulfide solid electrolyte, which affects the electrochemical properties of the sulfide solid electrolyte.

[0054] Although Comparative Example 3 used a secondary sintering process, no sintering aid was added during the secondary sintering process, so the mixture did not completely form Li6PS5Cl, reducing the content of effective ingredients that actually play a role in the sulfide solid electrolyte and affecting the electrochemical properties of the sulfide solid electrolyte.

[0055] Although the secondary sintering process was used in Comparative Example 4, the rotary sintering process was not used in the secondary sintering, which resulted in a larger particle size of the primary particles, affecting the electrochemical properties of the sulfide solid electrolyte.

[0056] The beneficial effects of the sulfide solid electrolyte and the preparation method thereof provided in this application include but are not limited to the following: 1) The sulfide solid electrolyte provided in the present application has a primary particle size D90≤2μm and a hardness lower than 120HB. The low-hardness sulfide solid electrolyte is used to prepare a highly densified sulfide solid electrolyte layer and improve the solid-solid interface, thereby improving battery performance.

[0057] 2) This application performs step-by-step sintering on the raw materials of the sulfide solid electrolyte, so that the raw materials can nucleate at a lower temperature, reducing the particle size of the primary particles, which is beneficial to reducing the hardness of the electrolyte, and the lower sintering temperature is also beneficial to reducing energy consumption.

[0058] 3) The secondary sintering of the present application is rotary sintering. The dynamic process of rotary sintering can effectively inhibit the agglomeration of primary particles of the material and reduce the particle size of secondary particles, thereby obtaining a sulfide solid electrolyte with small particle size and low hardness.

[0059] In summary, after reading the contents of this application, those skilled in the art will appreciate that the aforementioned application contents may be presented only in an exemplary manner and may not be restrictive. Although not explicitly stated herein, those skilled in the art will appreciate that this application is intended to encompass various reasonable changes, improvements and modifications to the embodiments. These changes, improvements and modifications are within the spirit and scope of the exemplary embodiments of this application.

Claims

1. A method for preparing a sulfide solid electrolyte, characterized in that: include: Mix Li2S, P2S5 and LiCl uniformly to obtain a first mixture; sintering the first mixture once, and obtaining an intermediate sintered product after cooling; mixing the intermediate sintered product with a sintering aid to obtain a second mixture; and performing secondary sintering on the second mixture and obtaining the sulfide solid electrolyte after cooling; Wherein, the particle size D90 of the primary particles of the sulfide electrolyte is ≤2 μm, and the hardness of the sulfide solid electrolyte is lower than 120 HB; In powder X-ray diffraction using CuKα rays, the sulfide solid electrolyte has diffraction peaks at 2θ=25.2±0.5 degrees and 29.7±0.5 degrees.

2. The preparation method according to claim 1, characterized in that The primary sintering temperature is 150-280° C. and the primary sintering time is 2-10 h.

3. The preparation method according to claim 1, characterized in that The temperature of the secondary sintering is 300-400° C.; the duration of the secondary sintering is 2-10 h.

4. The preparation method according to claim 1, characterized in that The secondary sintering is rotary sintering; the linear speed of the rotary sintering is 0.5-5 m / min.

5. The preparation method according to claim 1, characterized in that: The sintering aid includes at least one of Li2S, Li2O, P2O5, P2S5, BaO, CaO, MgO, TiO2, SiO2, Al2O3, ZnO, and Y2O3.

6. The preparation method according to claim 1, characterized in that: By weight, the sintering aid is 0.2%-1.0wt% of the intermediate sintered product.

7. The preparation method according to claim 1, characterized in that The mixing of the intermediate sintered product and the sintering aid comprises: crushing the intermediate sintered product; and The crushed intermediate sintered product is mixed with the sintering aid.

8. A sulfide solid electrolyte, characterized in that: The particle size D90 of primary particles of the sulfide solid electrolyte is ≤2 μm, and the hardness of the sulfide solid electrolyte is less than 120 HB; in powder X-ray diffraction using CuKα rays, the sulfide solid electrolyte has diffraction peaks at 2θ=25.2±0.5 deg and 29.7±0.5 deg.

9. A battery, characterized in that: It comprises a sulfide solid electrolyte prepared by the preparation method of any one of claims 1 to 7 or a sulfide solid electrolyte as claimed in claim 8.