Hard carbon material with adjustable pore structure as well as preparation method and application of hard carbon material
The precursor is formed by reacting organic amines and oxalic acid, and polymerization and high-temperature carbonization form hard carbon materials, solving the performance problems of hard carbon materials in sodium ion batteries and achieving the adjustment of pore structure and improving performance.
Patent Information
- Application Number
- CN202310626674.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing hard carbon materials have low first-time Coulomb efficiency, poor rate performance and long cycle stability in sodium ion batteries, and the complex pore making steps lead to difficulty in regulating the pore structure.
The reaction of organic amine molecules and oxalic acid to form a precursor, polymerization and high-temperature carbonization are carried out, and the low-temperature decomposition of oxalic acid is used to generate an open pore structure, and closed in the carbonization process to form a closed pore structure, avoid the pickling step, simplify the preparation process and optimize the pore structure .
The rate performance and cycle stability of hard carbon materials are improved, the preparation steps are simplified, and the excellent pore-making effect and material performance of the pore structure are achieved.
Smart Images

Figure CN119059510A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hard carbon materials, and relates to a hard carbon material with adjustable pore structure, a preparation method thereof, and application of the hard carbon material in a sodium ion battery. Background Art
[0002] Sodium-ion batteries have become a new research hotspot due to their rich sodium content and low cost. Although sodium and lithium have similar physical / chemical properties, the radius of sodium ions is larger than that of lithium ions, which makes graphite, a commercial lithium-ion negative electrode material, unable to store sodium ions. This has become the main challenge in the development of sodium-ion batteries. Compared with graphite materials, hard carbon materials have a larger interlayer spacing, which can ensure the insertion of sodium ions. They are also cheap, easy to obtain, safe, non-toxic and environmentally friendly. They are considered to be the most promising negative electrode materials for sodium-ion batteries. However, current hard carbon materials still face problems such as low first coulomb efficiency, poor rate performance and long-cycle stability. In order to better realize commercial applications, in-depth research is needed.
[0003] The study found that the capacity of the slope and platform regions of hard carbon materials for sodium storage is related to surface defects and internal closed pores, respectively. The platform capacity is the main contributor to the total capacity of the carbon anode, so closed pores are the main microstructure responsible for sodium storage.
[0004] Chinese patent document CN115676804A discloses a porous hard carbon negative electrode material based on asphalt, and its preparation method and application, in which asphalt powder is modified by a crosslinking agent or a modifier, and then a metal salt pore-forming agent is added, and then a porous hard carbon material is obtained by subsequent high-temperature carbonization and acid washing. The method can obtain a hard carbon material with a highly disordered and spherical multi-porous structure, but the subsequent acid washing requires cumbersome steps, and the addition of an activator consumes carbon, resulting in low yield. Summary of the invention
[0005] In order to improve the performance problems of low first coulomb efficiency, poor rate performance and long cycle stability of hard carbon materials prepared by prior art, as well as the problem that the pore-forming steps of current hard carbon materials are complicated and the pore structure is difficult to control, the present invention provides a hard carbon material with adjustable pore structure and its preparation method and use, wherein the method is to generate a precursor by reacting an organic amine molecule and oxalic acid, and then polymerize and carbonize the precursor at high temperature to prepare the hard carbon material. The present invention generates gaseous components such as water vapor, CO and CO2 by low-temperature decomposition of oxalic acid at about 189°C to form an open pore structure in the precursor, and then closes the formed open pores to generate a closed-pore structure through high-temperature carbonization. The prepared hard carbon material does not require a subsequent pickling process, has simple steps, and has excellent pore-forming effect. In addition, hard carbon materials with different pore structures can be prepared by adjusting the feed ratio of organic amine molecules and oxalic acid, selecting different organic amine molecules and carbonization temperatures.
[0006] The object of the present invention is achieved through the following technical solutions:
[0007] A method for preparing a hard carbon material, the method comprising the following steps:
[0008] (1) mixing an organic amine molecule and oxalic acid, reacting them, and preparing a precursor;
[0009] (2) subjecting the precursor of step (1) to a polymerization reaction, and then carbonizing the polymerization product under an inert atmosphere or a reducing atmosphere to prepare the hard carbon material.
[0010] According to an embodiment of the present invention, in step (1), the organic amine molecule is selected from compounds containing amino functional groups or amine functional groups. Exemplarily, the organic amine molecule is selected from one, two or more of aliphatic amine compounds and their derivatives, aromatic amine compounds and their derivatives, naphthylamine compounds and their derivatives, amide compounds and their derivatives, alcoholamine compounds and their derivatives, and amino compounds and their derivatives.
[0011] Exemplarily, the organic amine molecule is selected from aniline, diphenylamine, triphenylamine, N-methylaniline, N-ethylaniline, 4-ethylaniline, o-toluidine, m-toluidine, p-toluidine, 2,5-dimethylaniline, 2,6-dimethylaniline, 3,5-dimethylaniline, p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, diaminodiphenylmethane, 3,3',5,5'-tetramethylbenzidine, N-methyl-1,2-phenylenediamine , dopamine, 1-aminopyridine, 2-aminopyridine, 3-aminopyridine, 1-aminopyrrole, 2-aminopyrrole, 3-aminopyrrole, o-aminophenol, p-aminophenol, m-aminophenol, p-aminobenzoic acid, 4-aminophthalic acid, 3,5-diaminobenzenesulfonic acid, 2,4-diaminobenzoic acid, p-aminobenzenesulfonic acid, p-aminophenylboric acid, p-aminophenylphosphoric acid, amino acids, urea and thiourea, etc., one, two or more thereof.
[0012] According to an embodiment of the present invention, in step (1), the mass ratio of the organic amine molecule to oxalic acid is 1:0.1 to 6, such as 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5 or 1:6.
[0013] According to an embodiment of the present invention, in step (1), the precursor may be one, two or more organic amine molecules mixed simultaneously and then reacted with oxalic acid; or each organic amine molecule is mixed with oxalic acid separately and then mixed together to obtain the precursor; or one, two or more organic amine molecules are mixed first and then reacted with oxalic acid, and then another one, two or more organic amine molecules are added to react.
[0014] According to an embodiment of the present invention, in step (1), the organic amine molecule and the oxalic acid may react in the presence of a solvent or in the absence of a solvent.
[0015] Illustratively, the reaction in the absence of a solvent is, for example, that the organic amine molecules and oxalic acid are reacted by dry mixing by grinding, ball milling, blender or crusher; such as the organic amine molecules and oxalic acid are dry mixed by grinding, ball milling, blender or crusher until no obvious particles are present.
[0016] Wherein, the grinding is performed by using a mortar, and the grinding time is 0.1h to 24h.
[0017] Wherein, the rotation speed of the ball mill is 5 to 1500 RPM, and the time of the ball mill is 0.1 h to 24 h.
[0018] Wherein, the rotation speed of the stirrer is 5 to 1500 RPM, and the stirring time is 0.1 h to 24 h.
[0019] Wherein, the rotation speed of the pulverizer is 5 to 20,000 RPM, and the pulverization time is 0.1 h to 24 h.
[0020] Exemplarily, the reaction in the presence of a solvent is, for example, mixing a solvent, an organic amine molecule and oxalic acid, and reacting. The mixing method is not particularly defined, and the mixing of the solvent, the organic amine molecule and the oxalic acid can be achieved. For example, the organic amine molecule and the oxalic acid can be dissolved in a solvent respectively, and then the two are mixed in any order (for example, the organic amine molecule solution is added to the oxalic acid solution, or the oxalic acid solution is added to the organic amine molecule solution); one of the organic amine molecule or the oxalic acid can be dissolved in a solvent first, and then the other of the organic amine molecule or the oxalic acid is added thereto; the organic amine molecule and the oxalic acid can be mixed first, and then the solvent is added.
[0021] Preferably, the solvent is one or a mixture of any of an organic solvent and water. For example, the organic solvent may be one, two or more of methanol, ethanol, propanol, toluene, acetone, isopropanol, NMP (N-methylpyrrolidone), DMF (N,N-dimethylformamide), DMSO (dimethyl sulfoxide), THF (tetrahydrofuran), benzene, toluene, xylene, pentane, hexane, octane, cyclohexane, cyclohexanone, ether, propylene oxide, methyl acetate, ethyl acetate, propyl acetate, methyl butyl ketone, methyl isobutyl ketone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, acetonitrile, phenol, toluene cyclohexanone, chlorobenzene, dichlorobenzene, dichloromethane, chloroform, carbon tetrachloride, etc.
[0022] Preferably, the ratio of the sum of the masses of the organic amine molecules and oxalic acid to the amount of the solvent is 1g:(1-100)mL, such as 1g:1mL, 1g:5mL, 1g:10mL, 1g:15mL, 1g:20mL, 1g:25mL, 1g:30mL, 1g:35mL, 1g:40mL, 1g:45mL, 1g:50mL, 1g:55mL, 1g:60mL, 1g:65mL, 1g:70mL, 1g:75mL, 1g:80mL, 1g:85mL, 1g:90mL, 1g:95mL or 1g:100mL.
[0023] Preferably, the organic amine molecules and oxalic acid before the reaction can be added by dripping with a dropper, dripping with a peristaltic pump, etc. For example, the addition method can be a peristaltic pump dropwise addition method. The addition speed is 0.1 to 200 mL / min.
[0024] According to an embodiment of the present invention, in step (1), the reaction is carried out under stirring, and the stirring can be carried out by mechanical stirring, magnetic stirring, ultrasonic stirring, etc. For example, magnetic stirring can be used to mix the materials evenly. The speed of the magnetic stirring is 5 to 1500 RPM, and the stirring time is 0 h to 48 h.
[0025] According to an embodiment of the present invention, in step (1), the reaction is carried out at room temperature, or under heating conditions, or under high pressure heating conditions (i.e., hydrothermal reaction).
[0026] Exemplarily, the heating is performed by heating in a water bath or an oil bath; the high-pressure heating is performed by performing a hydrothermal reaction in a stirred reactor, a solvent thermal reactor, a hydrothermal reactor, a supercritical reactor or a microwave reactor.
[0027] According to an embodiment of the present invention, in step (1), the reaction time is 0.1 to 72 h; such as 5 h, 10 h, 15 h, 20 h, 25 h, 30 h, 35 h, 40 h, 45 h, 50 h, 55 h, 60 h, 65 h, 70 h or 72 h.
[0028] According to an embodiment of the present invention, in step (1), the reaction temperature is 20-350°C; such as 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C, 210°C, 220°C, 230°C, 240°C, 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 330°C, 340°C or 350°C.
[0029] According to an embodiment of the present invention, if the reaction is carried out at room temperature, the reaction temperature is 20-40°C; if the reaction is carried out under heating conditions, the reaction temperature is 50-250°C; if the reaction is carried out under high pressure heating conditions, the reaction temperature is 100-350°C.
[0030] According to an embodiment of the present invention, in step (1), the reaction mixture is separated, for example, by centrifugation, drying, filtering, etc.
[0031] Preferably, the centrifugation can be performed by a centrifuge; wherein the centrifugation speed is 5 to 20,000 RPM, and the centrifugation time is 1 min to 60 min.
[0032] Preferably, the drying can be performed by at least one of rotary evaporation drying, freeze drying, spray drying, forced air oven drying, vacuum oven drying, and the like.
[0033] Preferably, the filtration is performed by conventional industrial suction filtration.
[0034] Preferably, the present invention does not impose any particular limitation on the method of drying the sample after reaction separation. For example, the material may be dried in an oven.
[0035] According to an embodiment of the present invention, in step (2), the polymerization reaction is carried out in the presence of a polymerization oxidant, for example, in the presence of a solid polymerization oxidant, a liquid polymerization oxidant or a gaseous polymerization oxidant.
[0036] Preferably, when the polymerization oxidant is solid, the polymerization oxidant can be selected from one, two or more of ferric chloride, potassium permanganate, potassium ferrate, ammonium persulfate and potassium persulfate;
[0037] Preferably, when the polymerization oxidant is a liquid, the polymerization oxidant can be selected from one, two or more of hydrogen peroxide, peracetic acid, concentrated sulfuric acid and concentrated nitric acid;
[0038] Preferably, when the polymerization oxidant is a gas, the polymerization oxidant is selected from an atmosphere in which oxygen exists, such as a mixed atmosphere of oxygen and an inert atmosphere, or pure oxygen or air.
[0039] According to an embodiment of the present invention, in step (2), the polymerization reaction temperature is 0°C to 400°C, such as 0°C, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 150°C, 180°C, 200°C, 250°C, 280°C, 300°C, 320°C, 350°C, 380°C, 400°C; the polymerization reaction time is 0.1h to 24h, such as 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 10h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.
[0040] According to an embodiment of the present invention, in step (2), the heating rate of the polymerization reaction is 0.05°C to 20°C / min, such as 0.05°C / min, 0.1°C / min, 1°C / min, 2°C / min, 5°C / min, 10°C / min, 15°C / min, and 20°C / min.
[0041] According to an embodiment of the present invention, in step (2), the polymerization reaction can be carried out using a solid polymerization oxidant, a liquid polymerization oxidant or a gaseous polymerization oxidant alone, or the three can be combined in any manner (such as first carrying out the polymerization reaction in the presence of a solid polymerization oxidant and / or a liquid polymerization oxidant, and then continuing to carry out the polymerization reaction in the presence of a gaseous polymerization oxide; or first carrying out the polymerization reaction in the presence of a gaseous polymerization oxidant, and then continuing to carry out the polymerization reaction in the presence of a solid polymerization oxide and / or a liquid polymerization oxidant). In particular, when the polymerization reaction is carried out in the presence of a solid polymerization oxidant and / or a liquid polymerization oxidant, the polymerization reaction temperature is 0°C to 150°C; when the polymerization reaction is carried out in the presence of a gaseous polymerization oxidant, the polymerization reaction temperature is 150°C to 400°C.
[0042] According to an embodiment of the present invention, in step (2), the temperature of the carbonization treatment is 300°C to 2800°C, such as 300°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1100°C, 1200°C, 1400°C, 1800°C, 2000°C, 2 400°C or 2800°C; the carbonization treatment time is 0.1 to 24h, such as 0.1h, 0.3h, 0.5h, 0.7h, 0.9h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.
[0043] According to the embodiment of the present invention, in step (2), the heating method of the carbonization treatment is not particularly limited, for example, the temperature may be directly raised to the carbonization treatment temperature and kept warm, or it may be paused at an intermediate temperature and then gradually raised to the carbonization treatment temperature, or it may be directly raised from the polymerization reaction temperature to the carbonization treatment temperature. For example, the temperature may be directly raised from 20°C to 1300°C; or the temperature may be raised from 20°C to 900°C and kept warm for 2h, and then raised to 1300°C.
[0044] According to an embodiment of the present invention, in step (2), the heating rate of the carbonization treatment is 0.05°C to 20°C / min, such as 0.05°C / min, 0.1°C / min, 1°C / min, 2°C / min, 5°C / min, 10°C / min, 15°C / min or 20°C / min.
[0045] According to an embodiment of the present invention, in step (2), the inert atmosphere is one of nitrogen, argon, helium, ammonia, etc., or a mixture of any multiple thereof.
[0046] According to an embodiment of the present invention, in step (2), the reducing atmosphere is pure hydrogen, or a gas mixed with one or more of nitrogen, argon, helium, ammonia, etc.
[0047] The present invention also provides a hard carbon material prepared by the method.
[0048] According to an embodiment of the present invention, the hard carbon material is a hard carbon material with adjustable pore structure.
[0049] According to an embodiment of the present invention, the hard carbon material has a closed-pore structure, and the closed-pore structure is formed by closing open pores formed by low-temperature decomposition of oxalic acid during a carbonization process.
[0050] According to an embodiment of the present invention, the porosity of the hard carbon material is 1% to 80%, for example, 5% to 60%.
[0051] According to an embodiment of the present invention, the true density of the hard carbon material is 0.5 to 2.0 g / cm 3 .
[0052] According to an embodiment of the present invention, the specific surface area of the hard carbon material is 1 to 100 cm 2 / g.
[0053] According to an embodiment of the present invention, the interlayer distance of the hard carbon material is 0.37 nm to 0.46 nm.
[0054] According to an embodiment of the present invention, at least one dimension of the hard carbon material is 0.1 μm to 100 μm, such as at least two dimensions are 0.1 μm to 100 μm, such as three dimensions are 0.1 μm to 100 μm.
[0055] According to an embodiment of the present invention, the first coulombic efficiency of the hard carbon material is above 80%.
[0056] According to an embodiment of the present invention, the stable discharge capacity of the hard carbon material is above 250 mAh / g.
[0057] According to an embodiment of the present invention, the hard carbon material has a morphology of spherical particles, long strips, rods, a three-dimensional cross-linked structure or a sheet structure.
[0058] The present invention also provides application of the hard carbon material in energy storage.
[0059] According to an embodiment of the present invention, the hard carbon material is used in sodium ion battery energy storage.
[0060] Beneficial effects of the present invention:
[0061] The present invention provides a hard carbon material with adjustable pore structure, and a preparation method and application thereof. The existing method for regulating the pore structure of hard carbon materials is to form pores by adding metal salts as activators or adding hard templates. Compared with the existing methods, the present invention uses a precursor generated by the reaction of organic amine molecules and oxalic acid, and the precursor is polymerized and carbonized to prepare a hard carbon material with adjustable pore structure. The present invention forms pores by low-temperature decomposition of oxalic acid. The formed pores collapse to form a closed-cell structure during the carbonization process. The prepared hard carbon material does not require the subsequent acid washing process of conventional pore formation, the steps are simple, and the pore formation effect is excellent; and hard carbon materials with different pore structures can be prepared by regulating the feed ratio of organic amine molecules and oxalic acid and regulating the carbonization temperature, which can greatly improve the rate performance and cycle stability of current hard carbon materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 This is a SEM morphology of the hard carbon material with adjustable pore structure prepared in Example 1.
[0063] Figure 2 This is the SEM morphology of the hard carbon material prepared in Comparative Example 1.
[0064] Figure 3 This is a rate performance diagram of the hard carbon material with adjustable pore structure prepared in Example 1.
[0065] Figure 4 This is a long cycle stability diagram of the hard carbon material with adjustable pore structure prepared in Example 1.
[0066] Figure 5 This is the SEM morphology of the hard carbon material with adjustable pore structure prepared in Example 4.
[0067] Figure 6 This is the SEM morphology of the hard carbon material with adjustable pore structure prepared in Example 5. DETAILED DESCRIPTION
[0068] The preparation method of the present invention will be described in further detail below in conjunction with specific examples. It should be understood that the following examples are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0069] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.
[0070] Example 1
[0071] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0072] Step 1: Weigh 1.0 g of oxalic acid and 1.0 g of 3-aminopyrrole, mix the two in a beaker, add 25 mL of aqueous solution, and continue stirring for 24 hours to obtain a reaction product;
[0073] Step 2: Separate the above product by suction filtration, and then dry it in a forced air drying oven at 80°C for 24 hours to obtain a precursor;
[0074] Step 3: Keep the precursor at 200°C for 3 hours in an oxygen atmosphere at a heating rate of 4°C / min; then keep it at 900°C for 2 hours in a nitrogen atmosphere at a heating rate of 5°C / min; then gradually heat it to 1300°C and keep it for 2 hours to obtain the hard carbon material with adjustable pore structure. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0075] Figure 1 This is a SEM morphology picture of the hard carbon material with adjustable pore structure prepared in Example 1. It can be seen from the SEM picture that the hard carbon material with adjustable pore structure prepared in Example 1 presents a three-dimensional cross-linked network structure as a whole.
[0076] The hard carbon material with adjustable pore structure prepared in Example 1 was electrochemically tested by using a standard CR2032 button cell. The working electrode was prepared by coating the slurry on a copper foil. The slurry was composed of the electrode material (hard carbon material with adjustable pore structure), Ketjen black and PVDF dispersed in NMP solvent in a weight ratio of 8:1:1, and the loading of the electrode material was 1.0 g / cm 2 . Button cells were assembled using the prepared electrodes, metal lithium counter electrodes and glass fiber separators. The electrolyte was 1.0M NaPF6 and the organic solvent was DME. All cells were left to stand overnight before electrochemical measurements. Constant current discharge / charge tests were performed in the voltage range between 0.05 and 3.0 V. All specific capacities and specific energies were calculated based on the mass of the electrode material (hard carbon material with adjustable pore structure).
[0077] Figure 3 This is a rate performance diagram of the hard carbon material with adjustable pore structure prepared in Example 1. It can be seen from the figure that at a current density of 0.1A / g, the battery has a stable high specific capacity of 340mAh / g, and at a high current density of 5A / g, it also has a stable specific capacity of 230mAh / g, indicating that the material has excellent rate performance.
[0078] Figure 4This is a long cycle stability performance diagram of the hard carbon material with adjustable pore structure prepared in Example 1. It can be seen from the figure that at a current density of 2.0 A / g, the battery still retains 86% of the initial capacity after 300 cycles, indicating that the material has excellent cycle stability.
[0079] Comparative Example 1
[0080] The other operations were the same as in Example 1, except that oxalic acid was not added.
[0081] Figure 2 This is a SEM morphology of the hard carbon material prepared in Example 1. From the SEM, it can be seen that the hard carbon material prepared by the sample without adding oxalic acid presents a block structure of 20 μm in size as a whole, and there is no obvious pore structure on the surface, indicating that the addition of oxalic acid can regulate the structure of hard carbon, and since no oxalic acid is added, the hard carbon material does not have a closed-pore structure formed by the open channels formed by the low-temperature decomposition of oxalic acid and closed during the carbonization process.
[0082] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable specific capacity of 260mAh / g, and at a high current density of 5A / g, it had a specific capacity of 120mAh / g. At a current density of 2.0A / g, the battery retained 60% of its initial capacity after 300 cycles.
[0083] Example 2
[0084] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0085] Step 1: Weigh 0.5 g of oxalic acid and 1.0 g of 3-aminopyrrole, mix the two in a beaker, add 25 mL of aqueous solution, and continue stirring for 24 hours to obtain a reaction product;
[0086] Step 2: Separate the above product by suction filtration, and then dry it in a forced air drying oven at 80°C for 24 hours to obtain a precursor;
[0087] Step 3: Keep the precursor at 200°C for 3 hours in an oxygen atmosphere at a heating rate of 4°C / min; then keep it at 900°C for 2 hours in a nitrogen atmosphere at a heating rate of 5°C / min; then gradually heat it to 1300°C and keep it for 2 hours to obtain the hard carbon material with adjustable pore structure. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0088] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable high specific capacity of 295mAh / g, and at a high current density of 5A / g, it also had a stable specific capacity of 144mAh / g. At a current density of 2.0A / g, the battery retained 82% of its initial capacity after 300 cycles.
[0089] Example 3
[0090] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0091] Step 1: Weigh 1.5 g of oxalic acid and 1.0 g of 3-aminopyrrole, mix the two in a beaker, add 25 mL of aqueous solution, and continue stirring for 24 hours to obtain a reaction product;
[0092] Step 2: Separate the above product by suction filtration, and then dry it in a forced air drying oven at 80°C for 24 hours to obtain a precursor;
[0093] Step 3: Keep the precursor at 200°C for 3 hours in an oxygen atmosphere at a heating rate of 4°C / min; then keep it at 900°C for 2 hours in a nitrogen atmosphere at a heating rate of 5°C / min; then gradually heat it to 1300°C and keep it for 2 hours to obtain the hard carbon material with adjustable pore structure. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0094] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable high specific capacity of 355mAh / g, and at a high current density of 5A / g, it also had a stable specific capacity of 269mAh / g. At a current density of 2.0A / g, the battery retained 75% of its initial capacity after 300 cycles.
[0095] Example 4
[0096] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0097] Step 1: Weigh 1.0 g of oxalic acid and 1.0 g of p-phenylenediamine, dissolve them in 30 mL of aqueous solution respectively, and then use a peristaltic pump to drop the oxalic acid solution into the p-phenylenediamine solution at a feeding rate of 5 mL / min, and then continue stirring for 24 hours to obtain a reaction product;
[0098] Step 2: Separate the above product by suction filtration, and then dry it in a forced air drying oven at 60°C for 12 hours to obtain a precursor;
[0099] Step 3: Keep the above precursor at 200°C for 6 hours in an oxygen atmosphere at a heating rate of 4°C / min; then gradually heat it to 1300°C in a nitrogen atmosphere and keep it for 2 hours at a heating rate of 2°C / min, to obtain the hard carbon material with adjustable pore structure. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0100] Figure 5 This is a SEM morphology of the hard carbon material with adjustable pore structure prepared in Example 4. From the SEM image, it can be seen that the hard carbon material with adjustable pore structure prepared in Example 4 has a long rod-like structure of 50 μm in length and 5 μm in width as a whole, and the pore structure can be clearly seen on the surface.
[0101] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable high specific capacity of 305mAh / g, and at a high current density of 5A / g, it also had a stable specific capacity of 165mAh / g. At a current density of 2.0A / g, the battery retained 88% of its initial capacity after 300 cycles.
[0102] Example 5
[0103] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0104] Step 1: Weigh 2.5 g of oxalic acid and 2.1 g of m-phenylenediamine, mix the two and directly add 50 mL of aqueous solution, and continue stirring for 24 hours to obtain a reaction product;
[0105] Step 2: directly place the above solution in a forced air drying oven at 80°C and dry it for 24 hours, and evaporate the solution to obtain a precursor;
[0106] Step 3: Keep the precursor at 200°C for 5 hours in an oxygen atmosphere with a heating rate of 5°C / min; then keep it at 900°C for 2 hours in a nitrogen atmosphere with a heating rate of 5°C / min, and obtain the hard carbon material with adjustable pore structure. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0107] Figure 6 This is a SEM morphology picture of the hard carbon material with adjustable pore structure prepared in Example 5. As can be seen from the SEM picture, the hard carbon material with adjustable pore structure prepared in Example 5 presents a cross-linked long carbon flake structure as a whole.
[0108] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable high specific capacity of 270mAh / g, and at a high current density of 5A / g, it also had a stable specific capacity of 163mAh / g. At a current density of 2.0A / g, the battery retained 80% of its initial capacity after 300 cycles.
[0109] Example 6
[0110] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0111] Step 1: Weigh 2.0 g of oxalic acid and 1.7 g of p-aminobenzenesulfonic acid, and mill them in a ball mill for 24 hours at a speed of 400 RPM;
[0112] Step 2: Dry the ball-milled material in a forced air drying oven at 80°C for 24 hours to obtain a precursor;
[0113] Step 3: Keep the precursor at 200°C for 3 hours in an oxygen atmosphere at a heating rate of 4°C / min; then keep it at 900°C for 2 hours in a nitrogen atmosphere at a heating rate of 5°C / min; then gradually heat it to 1300°C and keep it for 2 hours to obtain the hard carbon material with adjustable pore structure. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0114] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable high specific capacity of 320mAh / g, and at a high current density of 5A / g, it also had a stable specific capacity of 178mAh / g. At a current density of 2.0A / g, the battery retained 80% of its initial capacity after 300 cycles.
[0115] Example 7
[0116] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0117] Step 1: Weigh 2.5 g of oxalic acid and 2.1 g of p-phenylenediamine, mix the two in a beaker, add 25 mL of aqueous solution, continue stirring for 24 hours to obtain a reaction product, then weigh 2.16 g of m-phenylenediamine, add it and continue stirring for 24 hours to obtain a reaction product;
[0118] Step 2: Separate the above product by suction filtration, and then dry it in a forced air drying oven at 60°C for 24 hours to obtain a precursor;
[0119] Step 3: Keep the above precursor at 200°C for 3 hours in an oxygen atmosphere at a heating rate of 4°C / min; then gradually heat it to 1300°C in a nitrogen atmosphere and keep it for 2 hours at a heating rate of 5°C / min; the hard carbon material with adjustable pore structure can be obtained. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0120] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable high specific capacity of 347mAh / g, and at a high current density of 5A / g, it also had a stable specific capacity of 266mAh / g. At a current density of 2.0A / g, the battery retained 83% of its initial capacity after 300 cycles.
[0121] Example 8
[0122] A method for preparing a hard carbon material with adjustable pore structure comprises the following steps:
[0123] Step 1: Weigh 1.0 g of oxalic acid and 2.0 g of 3,5-dimethylaniline, mix the two in a beaker, add 60 mL of aqueous solution, and then put them into a hydrothermal reactor, and hydrothermally heat at 100 ° C for 24 hours to obtain a reaction product;
[0124] Step 2: Using freeze drying to separate the above products to obtain the precursor;
[0125] Step 3: Keep the precursor at 200°C for 3 hours in an oxygen atmosphere at a heating rate of 4°C / min; then keep it at 900°C for 2 hours in a nitrogen atmosphere at a heating rate of 5°C / min; then gradually heat it to 1300°C and keep it for 2 hours to obtain the hard carbon material with adjustable pore structure. The prepared hard carbon material has a closed-pore structure, which is formed by the closure of open pores formed by low-temperature decomposition of oxalic acid during the carbonization process.
[0126] Using it as an electrode material, the battery was tested according to the test method of Example 1. At a current density of 0.1A / g, the battery had a stable high specific capacity of 312mAh / g, and at a high current density of 5A / g, it also had a stable specific capacity of 168mAh / g. At a current density of 2.0A / g, the battery retained 80% of its initial capacity after 300 cycles.
[0127] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a hard carbon material, the method comprising the following steps: (1) mixing an organic amine molecule and oxalic acid, reacting them, and preparing a precursor; (2) subjecting the precursor of step (1) to a polymerization reaction, and then carbonizing the polymerization product under an inert atmosphere or a reducing atmosphere to prepare the hard carbon material.
2. The preparation method according to claim 1, wherein In step (1), the organic amine molecules are selected from one, two or more of aliphatic amine compounds and their derivatives, aromatic amine compounds and their derivatives, naphthylamine compounds and their derivatives, amide compounds and their derivatives, alcoholamine compounds and their derivatives, and amino compounds and their derivatives. Preferably, the organic amine molecule is selected from aniline, diphenylamine, triphenylamine, N-methylaniline, N-ethylaniline, 4-ethylaniline, o-toluidine, m-toluidine, p-toluidine, 2,5-dimethylaniline, 2,6-dimethylaniline, 3,5-dimethylaniline, p-phenylenediamine, o-phenylenediamine, m-phenylenediamine, diaminodiphenylmethane, 3,3',5,5'-tetramethylbenzidine, N-methyl-1,2-phenylenediamine , dopamine, 1-aminopyridine, 2-aminopyridine, 3-aminopyridine, 1-aminopyrrole, 2-aminopyrrole, 3-aminopyrrole, o-aminophenol, p-aminophenol, m-aminophenol, p-aminobenzoic acid, 4-aminophthalic acid, 3,5-diaminobenzenesulfonic acid, 2,4-diaminobenzoic acid, p-aminobenzenesulfonic acid, p-aminophenylboric acid, p-aminophenylphosphoric acid, amino acids, urea and thiourea, etc., one, two or more thereof.
3. The preparation method according to claim 1 or 2, wherein In step (1), the mass ratio of the organic amine molecule to oxalic acid is 1:0.1-6.
4. The preparation method according to any one of claims 1 to 3, wherein: In step (1), the organic amine molecule and the oxalic acid may react in the presence of a solvent or in the absence of a solvent. Preferably, the reaction in the absence of a solvent is, for example, that the organic amine molecules and oxalic acid are reacted by dry mixing in a grinding, ball milling, blender or pulverizer. Preferably, the reaction in the presence of a solvent is, for example, mixing a solvent, an organic amine molecule and oxalic acid and reacting them. Preferably, the ratio of the sum of the masses of the organic amine molecules and oxalic acid to the solvent is 1 g: (1-100) mL.
5. The preparation method according to any one of claims 1 to 4, wherein: In step (1), the reaction is carried out at room temperature, under heating conditions, or by hydrothermal reaction. Preferably, in step (1), the reaction time is 0.1 to 72 hours. Preferably, in step (1), the reaction temperature is 20 to 350°C.
6. The preparation method according to any one of claims 1 to 5, wherein: In step (2), the polymerization reaction is carried out in the presence of a polymerization oxidant, and the polymerization oxidant is a solid polymerization oxidant, a liquid polymerization oxidant or a gaseous polymerization oxidant. Preferably, in step (2), the polymerization reaction temperature is 0°C to 400°C; and the polymerization reaction time is 0.1h to 24h.
7. The preparation method according to any one of claims 1 to 6, wherein: In step (2), the temperature of the carbonization treatment is 300° C. to 2800° C.; and the time of the carbonization treatment is 0.1 to 24 hours. Preferably, in step (2), the heating rate of the carbonization treatment is 0.05°C to 20°C / min.
8. A hard carbon material prepared by the method according to any one of claims 1 to 7.
9. The hard carbon material according to claim 8, wherein The hard carbon material has a closed-pore structure, and the closed-pore structure is formed by closing open pores formed by low-temperature decomposition of oxalic acid during a carbonization process. and / or, the porosity of the hard carbon material is 1% to 80%; And / or, the true density of the hard carbon material is 0.5-2.0 g / cm 3 ; And / or, the specific surface area of the hard carbon material is 1 to 100 cm 2 / g; and / or, the interlayer spacing of the hard carbon material is 0.37 nm to 0.46 nm; And / or, at least one dimension of the hard carbon material is 0.1 μm to 100 μm; And / or, the hard carbon material has a morphology of spherical particles, long strips, rods, a three-dimensional cross-linked structure or a sheet structure.
10. Application of the hard carbon material according to claim 8 or 9 in energy storage. Preferably, the hard carbon material is used in sodium ion battery energy storage.
Citation Information
Patent Citations
Preparation method of hydrophobic porous carbon material
CN112408360A
Method for preparing layered carbon material from small organic molecules and application of layered carbon material in energy storage
CN115818614A
Doped modified hard carbon material as well as preparation method and application thereof
CN115872388A