Method for removing magnesium oxide in high-magnesium limestone by synergistically utilizing ardealite
By carbonizing high-magnesium limestone and phosphogypsum, using CO2 gas, the removal of magnesium oxide in high-magnesium limestone and the resource utilization of phosphogypsum are achieved, and low-grade limestone and phosphogypsum are solved in silicate cement and low-carbon The problem of reducing active ingredients in cement production improves the cost-effectiveness of resource utilization and reduces the MgO content.
Patent Information
- Application Number
- CN202411188308.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to effectively utilize low-grade limestone and phosphogypsum, especially high-magnesium limestone, which leads to reduced active ingredients in silicate cement and low-carbon cement production, low cost-effectiveness in resource utilization, and complex phosphogypsum. The composition affects its resource utilization.
By synergistically utilizing phosphogypsum, high-magnesium limestone and phosphogypsum are mixed, mixed with water, and carbonized with CO2 gas, forming high-value limestone with low MgO content or no MgO, and synchronously obtaining high-purity MgSO4 , solid-liquid separation is performed by chemical reactions from reactions 1 to reaction 4, and the MgO content in the solid phase is reduced.
It has achieved efficient resource utilization of high-magnesium limestone and phosphogypsum, reduced MgO content, improved the active ingredients of silicate cement and low-carbohydrate cement, and has significant economic and environmental benefits, and is suitable for promotion and application.
Smart Images

Figure BDA0005014208010000041 
Figure BDA0005014208010000062 
Figure BDA0005014208010000063
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic non-metallic solid waste treatment, and specifically relates to a method for collaboratively utilizing phosphogypsum to remove magnesium oxide in high-magnesium limestone. Background Art
[0002] As one of the most widely distributed mineral resources in the earth's crust, limestone plays an irreplaceable role in many fields. In the manufacture of Portland cement, the limestone that can be used can be divided into primary and secondary grades. The CaO content of primary limestone is greater than 48% and the MgO content does not exceed 2.5%. The CaO content of secondary limestone is 45-48% and the MgO content does not exceed 3%. Limestone with low CaO content usually has high MgO content, mainly because dolomite is accompanied in the limestone. Excessive MgO content will increase the calcination temperature of Portland cement clinker, reduce the content of effective hydration active ingredients, and MgO will exist in the form of low-activity overburned MgO, which is difficult to meet the requirements of production and product standards. Therefore, most secondary limestone cannot be used as a raw material for calcining Portland cement clinker, and primary limestone is generally required.
[0003] In the manufacture of low-carbon cement, if low-grade limestone (high-magnesium limestone) is used to produce low-carbon cement clinker, MgO will enter into the highly active low-calcium-silicon ratio calcium silicate minerals C2S, C3S2, and CS to form less active C7MS4, C3MS2, and C2MS2. Moreover, since the relative molecular mass of MgO is significantly smaller than that of Al2O3, MgO can combine with more CaO and SiO2 (forming less active C7MS4, C3MS2, and C2MS2), thereby significantly reducing the carbonization activity of the low-carbon clinker.
[0004] In the existing manufacturing industry, low-grade limestone is usually crushed and used as concrete aggregate, or ground into stone powder for use as a mixed material in cement production and admixture in concrete, due to its high MgO content. However, different low-grade limestones have different ratios of CaCO3 and CaMg(CO3)2, and their chemical compositions are quite different. The performance is unstable when used, and the resource utilization is cost-effective, resulting in low economic and environmental benefits.
[0005] Phosphogypsum is a solid waste produced in the wet phosphoric acid process and is the biggest obstacle to the development of phosphorus chemical industry and new energy materials industry. The composition of phosphogypsum is relatively complex. In addition to hydrated calcium sulfate, there are also incompletely decomposed phosphate ore, residual phosphoric acid, fluoride, acid insoluble matter, organic matter, etc. Among them, the presence of fluorine and organic matter has the greatest impact on the resource utilization of phosphogypsum. Stacking will occupy a large amount of land and cause pollution to water and land resources.
[0006] How to effectively utilize low-grade limestone (high-magnesium limestone) and phosphogypsum, remove MgO and SO3 that are not conducive to the production of silicate cement and low-carbon cement, and convert them into more valuable substances has become a technical problem that needs to be solved urgently. Summary of the invention
[0007] The main purpose of the present invention is to provide a method for synergistically utilizing phosphogypsum to remove magnesium oxide in high-magnesium limestone, synergistically utilizing phosphogypsum to carbonize low-value limestone-based raw materials with high MgO content to form high-value limestone with low MgO content or without MgO, and at the same time produce MgSO4 with higher purity, which has significant social and economic benefits and is suitable for promotion and application.
[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:
[0009] A method for removing magnesium oxide from high-magnesium limestone by synergistically utilizing phosphogypsum comprises the following steps:
[0010] (1) drying and crushing high-magnesium limestone, and decomposing it in a lime kiln to obtain high-magnesium calcined material;
[0011] (2) mixing and grinding the high-magnesium calcined material and phosphogypsum to obtain a mixed material;
[0012] (3) adding water to the obtained mixture and stirring it into a slurry;
[0013] (4) continuously introducing CO2 gas into the slurry for carbonization;
[0014] (5) Filter the obtained carbonized product to obtain solid and liquid MgSO4 solution (filtrate).
[0015] According to the above scheme, the high-magnesium limestone is limestone particles, stone powder or aggregate waste slag with low CaO content and high MgO content, and its main chemical components and contents are: CaO 20-45%, MgO 5-20%, SiO2 4-30%, Al2O3 0-6%, Fe2O30-6%; loss on ignition 20-45%.
[0016] According to the above scheme, the chemical components and their mass percentages in the phosphogypsum include: SiO2 5-8%, Al2O3 0-1%, Fe2O3 0-1%, CaO 28-32%, MgO 0-1%, SO3 40-44%, K2O 0-1%, Na2O 0-1%; and the loss on ignition is 18-22%.
[0017] According to the above scheme, the calcination temperature of the lime kiln in step (1) is 750-900°C, and the calcination time is 5-20min.
[0018] According to the above scheme, the batching conditions in step (2) are: the molar ratio of MgO introduced into the chemical composition of the high-magnesium calcined material to SO3 introduced into the chemical composition of the phosphogypsum is 1:(0.5-1).
[0019] According to the above scheme, in the slurry described in step (3), the mass ratio of the mixture to water is 1:(5-50).
[0020] According to the above scheme, the carbonization method described in step (4) is: continuously stirring the slurry at a rotation speed of 100-500r / min and a temperature of 20-70°C, and then passing CO2 gas therein at a flow rate of 0.2-10m / s until the mass of the introduced CO2 reaches 1.1-5 times the mass of MgO in the slurry.
[0021] Furthermore, in the CO2 gas, the concentration of CO2 is 5-99 vol%.
[0022] Furthermore, the CO2 gas can be industrial CO2 tail gas or the like.
[0023] According to the above scheme, the solid phase obtained in step (5) is mainly composed of CaCO3 and SiO2 with low crystallinity after drying, and the content of MgO in its chemical composition is less than 2%, and the content of SO3 is less than 1%; it can be used in the fields of raw materials for the production of silicate clinker and low-carbon clinker, high-activity mixed materials and high-activity crystal seeds.
[0024] Preferably, the carbonization step adopts high temperature first and low temperature later, which can further increase the reaction rate, reduce the SO3 content and ensure the low MgO content; the high temperature condition is 50-70°C, and the low temperature condition is 20-40°C; the amount of gas introduced under the high temperature condition is more than half of the total gas amount.
[0025] According to the above scheme, the liquid phase in step (5) is mainly composed of MgSO4·6H2O after drying, and the content of CaO in the chemical composition does not exceed 1wt%.
[0026] The principle of the present invention is:
[0027] The reaction process of the present invention includes reaction 1 to reaction 4:
[0028] Reaction 1 is the digestion of MgO to form Mg(OH)2:
[0029] MgO+H2O→Mg(OH)2
[0030] Reaction 2 is the dissolution of CO2 in water:
[0031] CO2+H2O→H2CO3
[0032] Reaction 3 is the carbonization of Mg(OH)2 to Mg(HCO3)2:
[0033] Mg(OH)2+H2CO3→MgCO3+2H2O
[0034] MgCO3+H2CO3→Mg(HCO3)2
[0035] Total: Mg(OH)2+2H2CO3→Mg(HCO3)2+2H2O
[0036] Reaction 4 is the carbonization of CaSO4·2H2O by Mg(HCO3)2 into CaCO3 and MgSO4:
[0037] Mg(HCO3)2+CaSO4·2H2O→CaCO3+CO2+3H2O+MgSO4
[0038] (1) Simply using the carbonization method to obtain Mg(HCO3)2 and CaCO3 for solid-liquid separation will result in a high content of MgO remaining in the solid phase due to the instability of Mg(HCO3)2. The present invention adds phosphogypsum on the basis of separating MgO by the carbonization method, promotes the progress of reactions 1 to 3 through reaction 4, and obtains MgSO4 with better stability and easier solid-liquid separation, thereby reducing the content of MgO remaining in the solid phase; it can simultaneously achieve efficient resource utilization of high-magnesium limestone and phosphogypsum, and realize the separation of Mg and Ca in high-magnesium limestone and the separation of Ca and S in phosphogypsum.
[0039] (2) Since it is necessary to ensure a high desulfurization rate of CaSO4·2H2O in phosphogypsum and promote its conversion into CaCO3, the amount of MgO in the batch is excessive compared to SO3, and the obtained liquid phase is mainly MgSO4 solution, with a CaO content of no more than 1%, but containing a small amount of Mg(HCO3)2. A small amount of H2SO4 can be added later to observe the bubbles for purification. If an excessive amount of H2SO4 is added, MgCO3, MgO, and Mg(OH)2 can be added until the pH changes from acidic to neutral for purification. The obtained MgSO4 can be used as a raw material for magnesium sulfate cement, and can also be used as an admixture for low-carbon cement clinker (to promote carbonization and generate aragonite).
[0040] (3) High reaction temperature can significantly increase the rate of reaction 1 to reaction 4 and reduce the SO3 content in the solid phase. However, Mg(HCO3)2 is less stable as the temperature increases, which reduces the conversion rate of Mg(HCO3)2 in reaction 3 and increases the MgO content in the chemical composition of the solid phase. The present invention proposes a method of high-temperature carbonization followed by low-temperature carbonization, wherein the high temperature is 50-70°C and the low temperature is 20-40°C. High-temperature carbonization increases the reaction rate and reduces the SO3 content in the solid phase, and low-temperature carbonization converts excess Mg(OH)2 into more stable Mg(HCO3)2, thereby ensuring a low MgO content in the solid phase.
[0041] (4) The CO2 concentration in most industrial tail gas is 10-50 vol%, which can be used for carbonization reaction in the present invention.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] 1) The present invention uses high-magnesium limestone and phosphogypsum as main raw materials, and carbonizes low-value limestone-based raw materials with high MgO content (it is impossible to achieve effective reaction between high-magnesium calcined materials and phosphogypsum without introducing carbonization reaction conditions) to form high-value limestone with low MgO content or no MgO, which can simultaneously realize high-value resource application of low-quality raw materials or industrial waste such as high-magnesium limestone and phosphogypsum, and has significant economic and environmental benefits;
[0044] 2) The grain size of CaCO3 in the solid phase obtained by the present invention is much smaller than that of natural limestone, and the molar ratio of CaO to SiO2 is greater than 3, the content of MgO is less than 2%, and the content of SO3 is less than 1%. It can be used as a high-activity raw material for producing silicate cement clinker and low-carbon cement clinker, and can also be used as a high-activity admixture and high-activity seed, and has wide applicability;
[0045] 3) The treatment process involved in the present invention is relatively simple and easy to operate, and can effectively utilize most of the industrial tail gas (CO2 concentration is usually 10-50vol%), which is suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 The present invention provides a process flow chart for removing magnesium oxide from high-magnesium limestone by synergistically utilizing phosphogypsum.
[0047] Figure 2 XRD spectra of the solid phase products obtained in Examples 1 to 4 and Comparative Example 1 (the five spectra from bottom to top are respectively Example 1, Example 2, Example 3, Example 4, and Comparative Example 1).
[0048] Figure 3 XRD spectra of the liquid products obtained in Examples 1 to 4 and Comparative Example 1 (the five spectra from bottom to top are respectively Example 1, Example 2, Example 3, Example 4, and Comparative Example 1).
[0049] Figure 4 XRD spectrum of the solid phase product obtained in Comparative Example 2
[0050] Figure 5 XRD spectrum of the liquid product obtained in Comparative Example 2
[0051] Figure 6 SEM image of the solid phase product obtained in Example 1.
[0052] Figure 7 SEM image of the liquid product obtained in Example 1. DETAILED DESCRIPTION
[0053] The present invention is not limited to the above-mentioned embodiments. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention. The contents not described in detail in this specification belong to the prior art known to professional and technical personnel in this field.
[0054] The following are high-magnesium limestone and phosphogypsum used in the specific embodiments:
[0055] The chemical compositions of high-magnesium limestone and phosphogypsum used in the embodiment of the present invention are shown in Table 1, and are ground to R80μm≤20%:
[0056] Table 1 Chemical composition of raw materials (%)
[0057]
[0058] Example 1
[0059] A method for removing magnesium oxide from high-magnesium limestone by synergistically utilizing phosphogypsum comprises the following steps:
[0060] 1. Calcination and decomposition of high-magnesium limestone
[0061] Obtain high-magnesium limestone, dry and crush it to a particle size of no more than 20 mm, and then put it into a lime kiln for decomposition. The calcination temperature is 850°C and the calcination time is 15 minutes to obtain a high-magnesium calcined material;
[0062] 2. Ingredients
[0063] The MgO content in the high-magnesium calcined material is measured to be 16.18%. The ingredients are prepared according to the molar ratio of MgO in the chemical composition of the high-magnesium calcined material to SO3 in the chemical composition of the phosphogypsum of 1:0.8, that is, 100*16.18%*0.8*80 / (40*42.46%)=60.97 parts of phosphogypsum are added to every 100 parts of the high-magnesium calcined material, and the mixture is ground to R80μm=15% to obtain a mixed material;
[0064] 3. Prepare slurry
[0065] Take 100g of the mixture and add 2000g of water to obtain a slurry;
[0066] 4. Carbonization
[0067] The slurry is continuously stirred at a speed of 200 r / min at a temperature of 40°C and 20 vol% industrial CO2 tail gas is introduced at a flow rate of 0.5 m / s until the mass of the introduced CO2 reaches twice the mass of MgO in the slurry, wherein the mass of CO2 to be introduced is calculated to be 16.18*100*2 / (100+60.97)=20.10 g, and the volume of the industrial CO2 tail gas introduced (under standard conditions) is further calculated to be 20.10*22.4 / (44*20%)=51.16 L;
[0068] 5. Filter
[0069] After carbonization, the product is filtered. The solid product obtained after filtration is CaCO3 after MgO is removed, and the liquid product obtained is MgSO4 solution.
[0070] Example 2
[0071] A method for removing magnesium oxide from high-magnesium limestone by synergistically utilizing phosphogypsum comprises the following steps:
[0072] 1. Calcination and decomposition of high-magnesium limestone
[0073] Obtain high-magnesium limestone, dry and crush it to a particle size of no more than 20 mm, and then put it into a lime kiln for decomposition. The calcination temperature is 850°C and the calcination time is 15 minutes to obtain a high-magnesium calcined material;
[0074] 2. Ingredients
[0075] The MgO content in the high-magnesium calcined material is measured to be 16.18%. The ingredients are prepared according to the molar ratio of MgO in the chemical composition of the high-magnesium calcined material to SO3 in the chemical composition of the phosphogypsum of 1:0.7, that is, 100*16.18%*0.7*80 / (40*42.46%)=53.35 parts of phosphogypsum are added to every 100 parts of the high-magnesium calcined material, and the mixture is ground to R80μm=15% to obtain a mixed material;
[0076] 3. Prepare slurry
[0077] Take 100g of the mixture and add 3000g of water to obtain a slurry;
[0078] 4. Carbonization
[0079] The slurry is continuously stirred at a speed of 200 r / min at a temperature of 40°C and 20 vol% industrial CO2 tail gas is introduced at a flow rate of 0.5 m / s until the mass of the introduced CO2 reaches 2.5 times the mass of MgO in the slurry, wherein the mass of CO2 to be introduced is calculated to be 16.18*100*2.5 / (100+53.35)=26.38 g, and the volume of the industrial CO2 tail gas introduced (under standard conditions) is further calculated to be 26.38*22.4 / (44*20%)=67.15 L;
[0080] 5. Filter
[0081] After carbonization, the product is filtered. The solid product obtained after filtration is CaCO3 after MgO is removed, and the liquid product obtained is MgSO4 solution.
[0082] Example 3
[0083] A method for removing magnesium oxide from high-magnesium limestone by synergistically utilizing phosphogypsum is substantially the same as Example 1, except that the reaction temperature during carbonization is 60°C.
[0084] Example 4
[0085] A method for synergistically utilizing phosphogypsum to remove magnesium oxide in high-magnesium limestone, which is substantially the same as Example 1, except that the carbonization adopts a method of first high-temperature carbonization and then low-temperature carbonization, wherein the amount of gas introduced at high temperature is at least half of the total amount of gas: first, 40 L of industrial CO2 tail gas (under standard conditions) is introduced at a reaction temperature of 70°C, and then the reaction temperature is transferred to 30°C and 11.16 L of industrial CO2 tail gas (under standard conditions) is introduced.
[0086] Comparative Example 1
[0087] A method for removing magnesium oxide from high-magnesium limestone, which is different from Example 1 in that only high-magnesium calcined material is used for carbonization removal of magnesium, and no phosphogypsum is added.
[0088] Comparative Example 2
[0089] A method for removing magnesium oxide from high-magnesium limestone, which differs from Example 1 in that high-magnesium limestone that has not been calcined in a lime kiln is directly used to perform a carbonization reaction with phosphogypsum.
[0090] The solid products obtained in Examples 1 to 4 and Comparative Examples 1 and 2 were dried at 45°C, and the liquid products were dried at 105°C. The XRD patterns were analyzed by jade for quantitative mineral composition and grain size analysis of CaCO3. The results are as follows: Figure 2 , Figure 3 , Figure 4 , Figure 5 , as shown in Table 2 and Table 3.
[0091] Table 2 Mineral composition (%) and grain size of CaCO3
[0092]
[0093] Table 3 Mineral composition (%) and grain size of CaCO3 and CaMg(CO3)2
[0094]
[0095]
[0096] The solid phase was analyzed for chemical composition SiO2, Al2O3, Fe2O3, CaO, MgO, and SO3, and the liquid phase was analyzed for chemical composition CaO. The results are shown in Table 4.
[0097] Table 4 Chemical composition (%)
[0098]
[0099] The solid phase obtained in Examples 1, 2, 3, and 4 is mainly composed of CaCO3, with a mass ratio of total CaO to SiO2 of about 5, an MgO content of no more than 2%, and an SO3 content of no more than 1%, which is completely suitable for the production raw materials of silicate cement clinker and low-carbon cement clinker, and the average grain size of CaCO3 is only 20nm, which is much smaller than the 80nm or more of natural limestone, so that the activity is high and the decomposition temperature is low; the liquid phase obtained in Examples 1, 2, 3, and 4 is mainly composed of MgSO4, in which the CaO content is no more than 1%, which can be used as a raw material for magnesium sulfate cement, and can also be used as an additive for low-carbon cement clinker (to promote carbonization and generate aragonite); wherein, Example 4 further reduces the MgO and SO3 contents in the solid phase by the method of high-temperature carbonization followed by low-temperature carbonization; and at the same time, the separation of Mg and Ca in high-magnesium limestone and the separation of Ca and S in phosphogypsum are realized.
[0100] In Comparative Example 1, no phosphogypsum is added, and Mg(HCO3)2 and CaCO3 are obtained by carbonization method alone for solid-liquid separation. Since Mg(HCO3)2 is unstable, the residual MgO content in the solid phase is high, and since reaction 4 does not occur, the average grain size of CaCO3 is larger than that of Examples 1, 2, 3, and 4.
[0101] Comparative Example 2 directly uses high-magnesium limestone that has not been calcined in a lime kiln to react with phosphogypsum for carbonization. The solid phase still contains natural limestone and natural dolomite with large grain size and unreacted gypsum. MgSO4 does not appear in the liquid phase, but a small amount of CaSO4·2H2O is dissolved and filtered into the liquid phase. The natural dolomite in the high-magnesium limestone has high crystallinity, is difficult to dissolve, and has low activity. It cannot directly react with the slightly soluble CaSO4·2H2O in the phosphogypsum, and cannot be carbonized into Mg(HCO3)2 without calcination to further react with CaSO4·2H2O.
[0102] The above-mentioned embodiments are only preferred embodiments of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A method for removing magnesium oxide from high-magnesium limestone by synergistically utilizing phosphogypsum, characterized in that: The following steps are involved: (1) drying and crushing high-magnesium limestone, and decomposing it in a lime kiln to obtain high-magnesium calcined material; (2) mixing and grinding the high-magnesium calcined material and phosphogypsum to obtain a mixed material; (3) adding water to the obtained mixture and stirring it into a slurry; (4) continuously introducing CO2 gas into the slurry for carbonization; (5) Filter the obtained carbonized product to obtain solid and liquid MgSO4 solution (filtrate).
2. The method according to claim 1, characterized in that The main chemical components and contents of the high-magnesium limestone are: CaO 20-45%, MgO 5-20%, SiO2 4-30%, Al2O3 0-6%, Fe2O3 0-6%; and the ignition loss is 20-45%.
3. The method according to claim 1, characterized in that The chemical components and their mass percentages in the phosphogypsum include: SiO2 5-8%, Al2O3 0-1%, Fe2O3 0-1%, CaO 28-32%, MgO 0-1%, SO3 40-44%, K2O 0-1%, Na2O 0-1%; and the ignition loss is 18-22%.
4. The method according to claim 1, characterized in that: The calcination temperature of the lime kiln in step (1) is 750-900° C., and the calcination time is 5-20 min.
5. The method according to claim 1, characterized in that The batching conditions in step (2) are as follows: the molar ratio of MgO introduced into the chemical composition of the high-magnesium calcined material to SO3 introduced into the chemical composition of the phosphogypsum is 1:(0.5-1).
6. The method according to claim 1, characterized in that The carbonization method described in step (4) is: continuously stirring the slurry at a rotation speed of 100-500r / min and a temperature of 20-70°C, and then passing CO2 gas therein at a flow rate of 0.2-10m / s until the mass of the introduced CO2 reaches 1.1-5 times the mass of MgO in the slurry.
7. The method according to claim 1, characterized in that In CO2 gas, the concentration of CO2 is 5-99 vol%.
8. The method according to claim 1, characterized in that The solid phase obtained in step (5) is mainly composed of CaCO3 and SiO2 after drying, and the content of MgO in its chemical composition is less than 2% and the content of SO3 is less than 1%.
9. The method according to claim 1, characterized in that: After drying, the liquid phase in step (5) is mainly composed of MgSO4·6H2O, and the content of CaO in the chemical composition does not exceed 1wt%.