Nano cerium oxide and preparation method thereof
The preparation of nano cerium oxide particles through precipitation titration method and calcination steps has solved the problems of high cost and low efficiency of nano cerium oxide synthesis in the prior art, and achieved efficient and low-cost preparation of nano cerium oxide, and the crystal form is controllable.
Patent Information
- Application Number
- CN202411420811.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-03
AI Technical Summary
The prior art is difficult to synthesize nano cerium oxide particles at low cost and high efficiency, resulting in a complex and high cost.
Nano-cerium oxide particles are prepared by precipitation titration, carbonization and calcination steps, including temperature control of the cerium salt solution, addition of sodium polyacrylate and sodium hydroxide or ammonia water, adjusting the pH and temperature, followed by filtration, washing, drying and Calcination to produce nano cerium oxide particles.
The preparation of nano cerium oxide with simple operation, controllable crystal form and high yield is realized, which reduces the preparation cost and improves the preparation efficiency.
Smart Images

Figure CN119059549A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nano material preparation, and specifically relates to nano cerium oxide and a preparation method thereof. Background Art
[0002] Nano cerium oxide has excellent abrasive properties. Nano cerium oxide has fine particles, high hardness, and low friction coefficient, and can effectively remove metal surface residues, oxide scale, and scratches during polishing. In addition, cerium oxide has an inhibitory effect on metal oxidation and corrosion. For some metal materials that are prone to oxidation and rust, the use of cerium oxide polishing can enhance the corrosion resistance of the material. It is widely used in metal polishing fields such as automobiles, electrical appliances, clocks and watches, glasses, and electronic components.
[0003] There are many methods for synthesizing nano-cerium oxide materials, including high-temperature calcination method (CN115849430A, CN117861644A, CN115417443A), carbonization-calcination method (CN117776250A), sol-gel method, coprecipitation method and hydrothermal method, etc. However, how to synthesize nano-cerium oxide particles at low cost and high efficiency is a major challenge.
[0004] The invention prepares nano basic cerium carbonate from a cerium salt solution through processes such as precipitation, settling, and carbonization, and obtains nano cerium oxide particles through suction filtration, washing, drying, and calcination. The process realizes the synthesis of nano cerium oxide particles at low cost and high efficiency, and the process method is simple, the operation steps are few, the yield is high, and it is easy to promote commercially. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing controllable crystal nano-cerium oxide.
[0006] The invention prepares nano cerium oxide particles through simple steps of precipitation titration, carbonization, calcination, etc. The nano cerium oxide preparation method provided by the invention has the advantages of simple operation, controllable cerium oxide crystal form and high yield.
[0007] The nano cerium oxide and the preparation method thereof can controllably prepare the nano cerium oxide by precipitation titration method, and the specific steps are as follows:
[0008] 1) dissolving a cerium salt (cerium chloride, cerium nitrate or cerium acetate) in water and stirring to obtain a cerium salt solution;
[0009] 2) controlling the temperature of the cerium salt solution in step 1), adding sodium polyacrylate, dropping a precipitant such as sodium hydroxide or ammonia water, aging for 6-36 hours, and obtaining a cerium hydroxide slurry;
[0010] 3) The slurry prepared in step 2) is adjusted to a Baume degree of 8-11, the temperature is controlled below 25°C, carbonized with CO2 to a pH of 7-8, and the drying temperature is 120°C. Stir for 30 minutes, filter, wash, dry, grind, and sieve. The calcination temperature is 500°C and the calcination time is 4 hours to obtain nano cerium oxide particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0012] Figure 1 This is a SEM photo of nano-cerium oxide prepared in Example 1;
[0013] Figure 2 This is a SEM photo of nano-cerium oxide prepared in Example 2;
[0014] Figure 3 This is a SEM photograph of nano-cerium oxide prepared in Example 3. DETAILED DESCRIPTION
[0015] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto. A nano cerium oxide and a preparation method thereof, the specific implementation method is as follows:
[0016] Embodiment 1:
[0017] 1) Add 500g of cerium chloride solid into 1L of hot water to obtain CeCl3 solution, and stir and control the temperature to 60°C;
[0018] 2) Weigh 250 g of sodium hydroxide and place it in 500 mL of water, add it dropwise to the solution obtained in step 1), and add 5‰ sodium polyacrylate;
[0019] 3) aging the slurry obtained in step 2) for 24 hours to form a cerium hydroxide solution;
[0020] 4) The slurry in step 3) is sized to a Baume degree of 9, carbonized with CO2 to a pH of 7, and stirred for 30 minutes;
[0021] 5) The precipitate obtained in step 4) was filtered, washed, and dried at 120° C. for 4 h.
[0022] 6) The basic cerium carbonate solid obtained in step 5) is crushed, sieved, and calcined at 500° C. for 4 hours to obtain nano cerium oxide particles.
[0023] SEM test was performed on the nano-cerium oxide prepared in Example 1, and it can be seen that the nano-cerium oxide has a rod-like structure ( Figure 1 ). The amount of cerium chloride and other substances added was adjusted to complete the kilogram-level preparation process.
[0024] Embodiment 2:
[0025] 1) Add 500 g of cerium acetate solid into 1 L of hot water to obtain a cerium acetate solution, stir and control the temperature to 70°C, and add 2‰ sodium polyacrylate;
[0026] 2) Weigh 250g of ammonia water into 500mL of water and add dropwise to the ammonia solution obtained in step 1):
[0027] 3) adding ammonia water in step 2) dropwise to the slurry and aging for 24 hours;
[0028] 4) The slurry in step 3) is adjusted to a Baume degree of 8, carbonized with CO2 to a pH of 7.2, and stirred for 30 minutes;
[0029] 5) The precipitate obtained in step 4) was filtered, washed, and dried at 120° C. for 4 h.
[0030] 6) The basic cerium carbonate solid obtained in step 5) is crushed, sieved, and calcined at 500° C. for 4 hours to obtain nano cerium oxide particles.
[0031] The nano-cerium oxide prepared in Example 2 was subjected to SEM testing, and it can be seen that the nano-cerium oxide presents a spherical structure ( Figure 2 ). The amount of cerium acetate and other substances added was adjusted to complete the kilogram-level preparation process.
[0032] Embodiment 3:
[0033] 1) Add 500 g of cerium nitrate solid into 1 L of hot water to obtain a cerium nitrate solution, stir and control the temperature to 80°C, and add 0.5‰ sodium polyacrylate;
[0034] 2) Weigh 250 g of aqueous ammonia and place it in 500 mL of water, and add it dropwise to the aqueous ammonia solution obtained in step 1);
[0035] 3) adding ammonia water in step 2) dropwise to the slurry and aging for 24 hours;
[0036] 4) The slurry in step 3) is adjusted to a Baume degree of 11, carbonized with CO2 to a pH of 7.2, and stirred for 30 minutes;
[0037] 5) The precipitate obtained in step 4) was filtered, washed, and dried at 120° C. for 4 h.
[0038] 6) The basic cerium carbonate solid obtained in step 5) is crushed, sieved, and calcined at 500° C. for 4 hours to obtain nano cerium oxide particles.
[0039] The nano-cerium oxide prepared in Example 3 was subjected to SEM testing, and it can be seen that the cubic structure of the nano-cerium oxide ( Figure 3 ). The amount of cerium nitrate and other substances added was adjusted to complete the kilogram-level preparation process.
Claims
1. A nano cerium oxide and a preparation method thereof, characterized in that: The preparation method of the nano cerium oxide comprises: 1) dissolving cerium salt (cerium chloride, cerium nitrate or cerium acetate) in hot water at 50-80° C. and stirring to obtain a cerium salt solution; 2) adding 0.3‰-8‰ sodium polyacrylate to the cerium salt solution in step 1), dropping a precipitant, and aging for 6-36 hours to obtain a cerium hydroxide slurry; 3) The slurry obtained in step 2) is slurried, cooled to below 25° C., carbonized with CO2, stirred for 30 min, filtered, and the filter cake is washed, dried, ground, sieved, and calcined to obtain nano cerium oxide particles.
2. The preparation method according to claim 1, characterized in that: In step 1), the weight ratio of solid to water is 1:1.5-4.
5.
3. The preparation method according to claim 1, characterized in that: In step 2), the precipitant is sodium hydroxide or ammonia water.
4. The preparation method according to claim 1, characterized in that: In step 3), the pulping degree of Baume is adjusted to 8-11, the temperature is controlled below 25°C, CO2 is carbonized to pH=7-8, and the drying temperature is 120°C.
5. The preparation method according to claim 1, characterized in that: In step 3), the calcination temperature is 500° C. and the calcination time is 4-8 hours.
Citation Information
Cited By
Method for preparing cerium dioxide through incomplete precipitation coupling hydrothermal conversion
CN122126873A