Ferrite composite material as well as preparation method and application thereof

Through the composite and cosintering technology of ferrite materials and barium titanate, the natural resonance frequency and initial magnetic permeability of ferrite materials are regulated, and the problems of high magnetic loss and low natural resonance frequency of existing ferrite materials are solved. Ferrite composite materials with high Snoek product and low magnetic loss are achieved, suitable for high frequency electronic component applications.

CN119059567APending Publication Date: 2024-12-03GANJIANG INNOVATION ACAD CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411173406.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing ferrite materials cannot meet the needs of lower magnetic losses and higher natural resonance frequencies, resulting in lower Snoek product and unable to meet the performance requirements at high frequencies.

Method used

By recombining the ferrite material Ba2MgaFebO22 with barium titanate BaTiO3 in different proportions, adjusting the x value in the chemical formula, changing the crystal structure of the original Y-type ferrite, controlling the natural resonance frequency and initial magnetic permeability, achieving a higher level of Advantages of Snoek product and lower magnetic loss.

Benefits of technology

The high Snoek product and low magnetic loss of ferrite composite materials are achieved, suitable for high frequency applications, and uniform single-phase materials are obtained through co-sintering processes, suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119059567A_ABST
    Figure CN119059567A_ABST
Patent Text Reader

Abstract

The invention relates to a ferrite composite material and a preparation method and application thereof, the chemical formula of the ferrite composite material is xBa < 2 > Mg Fe O < 2 >. 3 BaTiO < 3 >, a ranges from 1.5 to 2.5, b ranges from 11.5 to 12.5, and x ranges from 1.1 to 2.0. The ferrite composite material provided by the invention is formed by compounding a ferrite material (Ba2MgaFebO22) and barium titanate (BaTiO3) in different proportions, the crystal structure of the original Y-type ferrite (Ba2MgaFebO22) is changed, and moreover, by regulating and controlling the value of x in the chemical formula of the ferrite composite material, the crystal structure of the Y-type ferrite (Ba2MgaFebO22) can be adjusted and controlled, so that the crystal structure of the Y-type ferrite (Ba2MgaFebO22) can be adjusted and controlled. The natural resonance frequency, the initial permeability and the magnetic loss of the ferrite material are controlled and adjusted, so that the ferrite composite material has the advantages of high Snoek product and low magnetic loss at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnetic materials, and in particular to a ferrite composite material and a preparation method and application thereof. Background Art

[0002] With the rapid development of microwave technology and the widespread integration of electronic communication equipment, the requirements for antennas are constantly moving towards high frequency and miniaturization. In recent decades, microstrip patch antennas have been favored due to their thin and planar characteristics. This planar structure is easy to manufacture using printed circuit technology and can be easily integrated into the surfaces of consumer products, aircraft, satellites and missiles, but its size, weight, cost, performance and installation convenience are still limiting factors.

[0003] For many years, people have been studying the use of high dielectric constant materials as substrate materials for microstrip patch antennas. However, high dielectric constant materials have two main disadvantages: first, the high concentration of the electric field in the high dielectric constant region leads to low antenna efficiency and narrow bandwidth; second, the low wave impedance of high dielectric constant materials leads to impedance matching difficulties.

[0004] In contrast, magneto-dielectric materials have significant advantages in miniaturizing antennas and improving efficiency due to their high refractive index, matching magnetic permeability and dielectric constant, and low magnetic loss and dielectric loss. The strong field confinement of magneto-dielectric materials reduces the occurrence of capacitive behavior problems that exist in high dielectric constant materials, and the approximately equivalent relative magnetic permeability and dielectric constant help to achieve impedance matching more easily. Ferrite materials, as a magneto-dielectric material, have attracted great attention in academia and industry and are regarded as important materials in the next generation of communications.

[0005] In response to the above problems, in order to adapt to the requirements of high frequency, integration, miniaturization and low power consumption of electronic components, it is necessary to increase the cutoff frequency and initial magnetic permeability of ferrite materials, and at the same time, it is necessary to increase the Snooker constant (also called Snoek product) of the material and reduce magnetic losses to obtain better performance.

[0006] CN110304913A discloses a high-frequency ultra-low loss manganese-zinc soft magnetic ferrite material and a preparation method thereof. The high-frequency ultra-low loss manganese-zinc soft magnetic ferrite material is composed of 140-146 parts by mass of Fe2O3, 39-48 parts by mass of Mn3O4, and 8-15 parts by mass of ZnO as main components. A trace amount of CaCO3, CoO, and Cr2O3 is added for the first time, and a trace amount of Y2O3, Sm2O3, SiO2, and V2O5 are added for the second time. The high-frequency ultra-low loss ferrite material is prepared by a solid phase method through batching, sand milling, doping, granulation, molding, and atmosphere sintering.

[0007] CN113744991 discloses a Co2Z type ferrite material and a preparation method and use thereof. A Y type mixed solution and an M type mixed solution are treated by electrodialysis to obtain a Y type cation mixed solution and an M type cation mixed solution. The Y type cation mixed solution and the M type cation mixed solution are mixed with ammonium bicarbonate, respectively, and dried to obtain a Y type ferrite precursor and an M type ferrite precursor. Finally, the Y type ferrite precursor, the M type ferrite precursor and a binder are pressed into shape, pre-sintered once, and sintered twice to obtain a Co2Z type ferrite material with uniform mixing, small particle size and high magnetic permeability.

[0008] However, the ferrite material disclosed in the above prior art cannot meet the demand for lower magnetic loss, and has a low natural resonance frequency, which ultimately leads to a low Snoek product of the material and cannot meet the performance requirements at higher frequencies.

[0009] Therefore, providing a ferrite material that can simultaneously have a high initial magnetic permeability and a high natural resonance frequency, so that the material has a high Snoek product and also has the advantage of low magnetic loss, is an issue that needs to be urgently addressed. Summary of the invention

[0010] In order to solve the above technical problems, the purpose of the present invention is to provide a ferrite composite material and its preparation method and application. The ferrite composite material provided by the present invention is composed of ferrite materials (Ba2Mg a Fe b O 22 ) and barium titanate (BaTiO3) composite, the original Y-type ferrite (Ba2Mg a Fe b O 22 )’s crystal structure is changed, and by adjusting the value of x in the chemical formula of the ferrite composite material, the natural resonance frequency, initial magnetic permeability and magnetic loss of the ferrite material are controlled and regulated, so that the ferrite composite material can have the advantages of both higher Snoek product and lower magnetic loss.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] In a first aspect, the present invention provides a ferrite composite material, wherein the chemical formula of the ferrite composite material is xBa2Mg a Fe b O 22 3BaTiO3, wherein a is 1.5-2.5, b is 11.5-12.5, and x is 1.1-2.0.

[0013] Specifically, in the chemical formula of the ferrite composite material described in the present invention, a can be 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5, etc.; b can be 11.5, 11.6, 11.8, 12.0, 12.2, 12.4 or 12.5, etc.; x can be 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9 or 2.0, etc.; but it is not limited to the listed values, and other values ​​not listed within the above numerical range are also applicable.

[0014] The ferrite composite material provided by the present invention adopts ferrite material (Ba2Mg a Fe b O 22 ) and barium titanate (BaTiO3) in different proportions, and the crystal structure of the original Y-type ferrite is changed and optimized. The ferrite composite material of the present invention can adjust the value of x in the chemical formula to achieve control and regulation of the natural resonance frequency and initial magnetic permeability of the ferrite material. Since in the ferrite composite material, Snoek product = natural resonance frequency × initial magnetic permeability, therefore, the present application can adjust the natural resonance frequency and initial magnetic permeability of the ferrite material within a higher range by adjusting the value of x in the chemical formula of the ferrite composite material, so that the ferrite composite material can have a higher Snoek product. In addition, the ferrite composite material with a specific composition in the present invention can also effectively reduce the magnetic loss of the ferrite material through the design of parameters.

[0015] In the present invention, if the x value is too low, although the natural resonance frequency of the material will be increased, the initial magnetic permeability of the material will be significantly reduced, thereby making the Snoek product of the ferrite composite material lower, resulting in poor material performance; and if the x value is too high, although the initial magnetic permeability of the material will be increased, the natural resonance frequency of the material will be reduced too much, thereby also making the Snoek product of the ferrite composite material lower.

[0016] Preferably, the chemical formula of the ferrite composite material is xBa2Mg a Fe b O 22 ·3BaTiO3, wherein a is 1.5-2.5, b is 11.5-12.5, and x is 1.1-1.5.

[0017] Preferably, the particle size D50 of the ferrite composite material is 0.5-5 μm, for example, 0.5 μm, 0.6 μm, 0.8 μm, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm.

[0018] In the present invention, if the particle size D50 of the ferrite composite material is too small, it will affect the magnetocrystalline anisotropy field and the natural resonance frequency; if the particle size D50 is too large, it will cause an increase in magnetic loss.

[0019] Preferably, the ferrite composite material is an intercalation structure.

[0020] Preferably, the initial magnetic permeability of the ferrite composite material is 1.5-11.8, for example, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, 11.5 or 11.8, etc.

[0021] Preferably, the damping coefficient of the ferrite composite material is 0.1-0.73, for example, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7 or 0.73.

[0022] In a second aspect, the present invention provides a method for preparing the ferrite composite material as described in the first aspect, the preparation method comprising:

[0023] (1) A first barium source, a magnesium source and an iron source are first mixed and calcined to obtain Ba2Mg a Fe b O 22 Pre-burned material, where a is 1.5-2.5 and b is 11.5-12.5;

[0024] (2) The Ba2Mg a Fe b O 22 The pre-sintered material and BaTiO3 are mixed for a second time in a molar ratio of (1.1-2.0):3, and after a second calcination, the ferrite composite material is obtained.

[0025] Specifically, in the Ba2Mg a Fe b O 22 In the chemical formula of the pre-sintered material, a may be 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4 or 2.5, etc.; b may be 11.5, 11.6, 11.8, 11.9, 12.0, 12.2, 12.4 or 12.5, etc.; the Ba2Mg a Fe b O 22The molar ratio of the pre-sintered material to BaTiO3 can be 1.1:3, 1.2:3, 1.3:3, 1.4:3, 1.5:3, 1.6:3, 1.7:3, 1.8:3, 1.9:3 or 2.0:3, etc. However, it is not limited to the listed values, and other values ​​not listed in the above numerical range are also applicable.

[0026] The ferrite composite material of the present invention is prepared by co-sintering a Y-type ferrite material and barium titanate to form a ferrite phase with an intercalated structure. a Fe b O 22 The ratio of the pre-sintered material to BaTiO3 is adjusted to adjust the natural resonance frequency and initial magnetic permeability of the material and the magnetic loss of the material, thereby realizing the change and optimization of the crystal structure of the Y-type ferrite material, so that the ferrite composite material has the advantages of both a higher Snoek product and a lower magnetic loss. In addition, the present invention is conducive to obtaining a uniform single-phase material through a co-sintering process of the ferrite material and barium titanate. In addition, the preparation method adopted by the present invention is simple to operate and suitable for industrial production.

[0027] Preferably, the preparation method of BaTiO3 comprises:

[0028] The second barium source and the titanium source are mixed for the third time and calcined for the third time to obtain the BaTiO3.

[0029] In the present invention, Ba2Mg a Fe b O 22 The preparation of pre-sintered material and BaTiO3 is in no particular order.

[0030] Preferably, the first barium source and the second barium source independently include BaCO3 and / or BaO.

[0031] Preferably, the titanium source comprises TiO2.

[0032] Preferably, the magnesium source comprises MgO and / or MgCO3.

[0033] Preferably, the iron source includes any one of Fe2O3, Fe2(CO)3 or Fe(CH3COO)3 (ferric acetate) or a combination of at least two thereof.

[0034] Preferably, the Ba2Mg a Fe b O 22 The pre-burned material is Y-type ferrite material.

[0035] Preferably, the first mixing, the second mixing and the third mixing methods independently include any one of ball milling, vibration milling or stirring, preferably ball milling.

[0036] Preferably, the rotation speed of the first mixing is 600-1500rad / min, for example, 600rad / min, 700rad / min, 800rad / min, 900rad / min, 1000rad / min, 1100rad / min, 1200rad / min, 1300rad / min, 1400rad / min or 1500rad / min, etc.

[0037] Preferably, the first mixing time is 2-4 h, such as 2 h, 2.5 h, 3 h, 3.5 h or 4 h.

[0038] Preferably, a first solvent is also added during the first mixing process.

[0039] Preferably, the first mixed material is further dried.

[0040] In the present invention, the drying method is not limited, and it can be natural air drying or vacuum drying, and those skilled in the art can choose according to needs.

[0041] Preferably, the heating rate of the first calcination is 2-3°C / min, such as 2°C / min, 2.2°C / min, 2.4°C / min, 2.6°C / min, 2.8°C / min or 3°C / min.

[0042] Preferably, the temperature of the first calcination is 1100-1200°C, for example, 1100°C, 1110°C, 1120°C, 1130°C, 1140°C, 1150°C, 1160°C, 1190°C or 1200°C.

[0043] In the present invention, if the temperature of the first calcination is too low, the reaction cannot be complete, affecting the uniformity of the product after the second calcination. If the temperature of the first calcination is too high, impurities will be generated, increasing magnetic loss.

[0044] Preferably, the first calcination time is 3-5 h, such as 3 h, 3.5 h, 4 h, 4.5 h or 5 h.

[0045] Preferably, the rotation speed of the second mixing is 600-1500rad / min, for example, 600rad / min, 700rad / min, 800rad / min, 900rad / min, 1000rad / min, 1100rad / min, 1200rad / min, 1300rad / min, 1400rad / min or 1500rad / min, etc.

[0046] Preferably, the second mixing time is 2-4 h, such as 2 h, 2.5 h, 3 h, 3.5 h or 4 h.

[0047] Preferably, a second solvent is added during the second mixing process.

[0048] Preferably, the particle size D50 of the material obtained after the second mixing is 0.5-2 μm, for example, 0.5 μm, 0.8 μm, 1.1 μm, 1.4 μm, 1.7 μm or 2 μm.

[0049] Preferably, the second mixed material is further dried.

[0050] Preferably, the heating rate of the second calcination is 2-3°C / min, such as 2°C / min, 2.2°C / min, 2.4°C / min, 2.6°C / min, 2.8°C / min or 3°C / min.

[0051] Preferably, the temperature of the second calcination is 1150-1250°C, for example, 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C or 1250°C.

[0052] In the present invention, if the temperature of the second calcination is too low, the product cannot be completely obtained by reaction, so that there is still unreacted Ba2Mg in the system. a Fe b O 22 ferrite, thus failing to effectively reduce the damping coefficient in the composite material; if the temperature of the second calcination is too high, an impure phase will be formed, affecting the magnetic properties of the composite material.

[0053] Preferably, the second calcination time is 1-6 h, such as 1 h, 2 h, 3 h, 4 h, 5 h or 6 h.

[0054] Preferably, the rotation speed of the third mixing is 600-1500rad / min, for example, 600rad / min, 700rad / min, 800rad / min, 900rad / min, 1000rad / min, 1100rad / min, 1200rad / min, 1300rad / min, 1400rad / min or 1500rad / min, etc.

[0055] Preferably, the third mixing time is 2-4 h, for example, 2 h, 2.5 h, 3 h, 3.5 h or 4 h.

[0056] Preferably, a third solvent is added during the third mixing process.

[0057] Preferably, the first solvent, the second solvent and the third solvent independently comprise ethanol and / or water.

[0058] Preferably, the third mixed material is further dried.

[0059] Preferably, the heating rate of the third calcination is 2-3°C / min, for example, 2°C / min, 2.2°C / min, 2.4°C / min, 2.6°C / min, 2.8°C / min or 3°C / min.

[0060] Preferably, the temperature of the third calcination is 1000-1250°C, for example, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C or 1250°C.

[0061] Preferably, the third calcination time is 3-5 h, such as 3 h, 3.5 h, 4 h, 4.5 h or 5 h.

[0062] As a preferred technical solution of the present invention, the preparation method of the ferrite composite material comprises:

[0063] (1) mixing a first barium source, a magnesium source, an iron source and a first solvent for 2-4 hours at a mixing speed of 600-1500 rad / min, drying the mixed material, and then calcining it at 1100-1200° C. for 3-5 hours at a heating rate of 2-3° C. / min to obtain Ba2Mg a Fe b O 22 Pre-sintered material; wherein a is 1.5-2.5, b is 11.5-12.5, and the obtained Ba2Mg a Fe b O 22 The pre-burned material is Y-type ferrite material;

[0064] The second barium source, the titanium source and the third solvent are mixed for 2-4 hours at a mixing speed of 600-1500 rad / min, the mixed material is dried, and then calcined at 1000-1250° C. for 3-5 hours at a calcination heating rate of 2-3° C. / min to obtain a BaTiO3 pre-sintered material;

[0065] (2) The Ba2Mg a Fe b O 22 The pre-sintered material, the BaTiO3 pre-sintered material and the second solvent are mixed for 2-4 hours, wherein Ba2Mg a Fe b O 22 The molar ratio of the pre-sintered material and the BaTiO3 pre-sintered material is (1.1-2.0):3, the mixing speed is 600-1500rad / min, the particle size D50 of the mixed material is 0.5-2μm, the mixed material is dried, and then calcined at 1150-1250℃ for 1-6h, and the calcination heating rate is 2-3℃ / min to obtain the ferrite composite material.

[0066] In a third aspect, the present invention provides an application of the ferrite composite material as described in the first aspect, wherein the ferrite composite material is applied in electronic components.

[0067] Preferably, the electronic component comprises an antenna or a circulator.

[0068] Compared with the prior art, the present invention has at least the following beneficial effects:

[0069] (1) The ferrite composite material provided by the present invention adopts ferrite material (Ba2Mg a Fe b O 22 ) and barium titanate (BaTiO3) in different proportions, and the crystal structure of the original Y-type ferrite is changed and optimized. The ferrite composite material of the present invention can adjust the value of x in the chemical formula, so as to achieve the control and adjustment of the natural resonance frequency and initial magnetic permeability of the ferrite material. Since in the ferrite material, the Snoek product = natural resonance frequency × initial magnetic permeability, therefore, the present application can adjust the natural resonance frequency and initial magnetic permeability of the ferrite material within a suitable range by adjusting the value of x in the chemical formula of the ferrite composite material, so that the ferrite composite material can have a higher Snoek product. In addition, the ferrite composite material with a specific composition in the present invention can also effectively reduce the magnetic loss of the ferrite material through the design of parameters.

[0070] (2) The ferrite composite material of the present invention is prepared by co-sintering a Y-type ferrite material and barium titanate to form a ferrite phase with an intercalated structure. a Fe b O 22 The ratio of the pre-sintered material to BaTiO3 is adjusted to adjust the natural resonance frequency and initial magnetic permeability of the material and the magnetic loss of the material, thereby realizing the change and optimization of the crystal structure of the Y-type ferrite material, so that the ferrite composite material has the advantages of both a higher Snoek product and a lower magnetic loss. In addition, the present invention is conducive to obtaining a uniform single-phase material through a co-sintering process of the ferrite material and barium titanate. In addition, the preparation method adopted by the present invention is simple to operate and suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 This is the magnetic permeability spectrum of the ferrite material obtained in Example 1 of the present invention.

[0072] Figure 2 This is the magnetic permeability spectrum of the ferrite material obtained in Example 4 of the present invention.

[0073] Figure 3 This is the magnetic permeability spectrum of the ferrite material obtained in Example 5 of the present invention. DETAILED DESCRIPTION

[0074] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0075] Example 1

[0076] This embodiment provides a ferrite composite material, whose chemical formula is 1.25Ba2Mg2Fe 12 O 22 ·3BaTiO3, particle size D50 is 3μm, and the structure is intercalation structure.

[0077] This embodiment also provides a method for preparing the above ferrite composite material, the preparation method comprising:

[0078] (1) 6.88 g of BaCO3, 16.71 g of Fe2O3 and 1.40 g of MgO were weighed and mixed with 140 mL of anhydrous ethanol, and ball milled on a planetary ball mill at a speed of 800 rad / min for 4 h. The ball milled material was vacuum dried and then calcined in a muffle furnace at a heating rate of 3 °C / min at a temperature of 1100 °C for 4 h to obtain Y-type Ba2Mg2Fe 12 O22 Pre-burned materials;

[0079] Weigh 8.26 g of BaCO3, 3.34 g of TiO2 and mix with 70 mL of anhydrous ethanol, and perform ball milling on a planetary ball mill at a speed of 800 rad / min for 4 h. The ball milled material is vacuum dried and then calcined in a muffle furnace at a heating rate of 3 ° C / min, a calcination temperature of 1100 ° C, and a time of 4 h to obtain BaTiO3 pre-sintered material;

[0080] (2) Weigh Ba2Mg2Fe in a molar ratio of 1.25:3 12 O 22 The pre-sintered material and BaTiO3 pre-sintered material were mixed with 200 mL of anhydrous ethanol and ball-milled in a planetary ball mill at a speed of 800 rad / min for 4 h. The particle size D50 of the mixed pre-sintered material after ball milling was 2 μm. The ball-milled material was vacuum dried and then calcined in a muffle furnace at a heating rate of 3 °C / min, a calcination temperature of 1200 °C, and a time of 4 h to obtain 1.25Ba2Mg2Fe 12 O 22 ·3BaTiO3 ferrite composite material.

[0081] The magnetic permeability spectrum of the ferrite composite material provided in this embodiment is as follows Figure 1 As can be seen from the figure, 1.25Ba2Mg2Fe 12 O 22 ·3BaTiO3 ferrite composite material has higher initial permeability, narrower natural resonance linewidth and lower imaginary part of permeability.

[0082] Example 2

[0083] This embodiment provides a ferrite composite material, whose chemical formula is 1.25Ba2Mg 1.5 Fe 12.5 O 22 ·3BaTiO3, particle size D50 is 4μm, and the structure is intercalated structure.

[0084] This embodiment also provides a method for preparing the above ferrite composite material, the preparation method comprising:

[0085] (1) 6.88 g of BaCO3, 17.40 g of Fe2O3 and 1.05 g of MgO were weighed and mixed with 140 mL of anhydrous ethanol, and ball milled on a planetary ball mill at a speed of 600 rad / min for 3 h. The ball milled material was vacuum dried and then calcined in a muffle furnace at a heating rate of 2 °C / min at a temperature of 1200 °C for 3 h to obtain Y-type Ba2Mg 1.5 Fe 12.5 O 22 Pre-burned materials;

[0086] Weigh 8.17 g of BaCO3, 3.31 g of TiO2 and 70 mL of anhydrous ethanol, and mix them. Mill them on a planetary ball mill at a speed of 700 rad / min for 4 h. Dry the milled material in a vacuum oven and calcine it in a muffle furnace at a heating rate of 3 °C / min at a temperature of 1150 °C for 4 h to obtain a BaTiO3 pre-sintered material.

[0087] (2) Weigh Ba2Mg in a molar ratio of 1.25:3 1.5 Fe 12.5 O 22 The pre-sintered material and the BaTiO3 pre-sintered material were mixed with 200 mL of anhydrous ethanol and ball-milled in a planetary ball mill at a speed of 1400 rad / min for 4 h. The particle size D50 of the mixed pre-sintered material after ball milling was 1 μm. The ball-milled material was vacuum dried and then calcined in a muffle furnace at a heating rate of 3 ° C / min, a calcination temperature of 1250 ° C, and a time of 2 h to obtain 1.25Ba2Mg 1.5 Fe 12.5 O 22 ·3BaTiO3 ferrite composite material.

[0088] Example 3

[0089] This embodiment provides a ferrite composite material, whose chemical formula is 1.25Ba2Mg 2.5 Fe 11.5 O 22 ·3BaTiO3, particle size D50 is 4μm, and the structure is intercalated structure.

[0090] This embodiment also provides a method for preparing the above ferrite composite material, the preparation method comprising:

[0091] (1) 6.88 g of BaCO3, 16.02 g of Fe2O3 and 1.74 g of MgO were weighed and mixed with 140 mL of anhydrous ethanol, and ball milled on a planetary ball mill at a speed of 1200 rad / min for 2 h. The ball milled material was vacuum dried and then calcined in a muffle furnace at a heating rate of 3 °C / min, a calcination temperature of 1150 °C, and a calcination time of 5 h to obtain Y-type Ba2Mg 2.5 Fe 11.5 O 22 Pre-burned materials;

[0092] Weigh 8.56 g of BaCO3, 3.46 g of TiO2 and mix with 70 mL of anhydrous ethanol, and perform ball milling on a planetary ball mill at a speed of 1300 rad / min for 3 h. The ball milled material is vacuum dried and then calcined in a muffle furnace at a heating rate of 2 ° C / min, a calcination temperature of 1200 ° C, and a time of 3 h to obtain BaTiO3 pre-sintered material;

[0093] (2) Weigh Ba2Mg in a molar ratio of 1.25:3 2.5 Fe 11.5 O 22 The pre-sintered material and the BaTiO3 pre-sintered material were mixed with 200 mL of anhydrous ethanol and ball-milled in a planetary ball mill at a speed of 600 rad / min for 4 h. The particle size D50 of the mixed pre-sintered material after ball milling was 2 μm. The ball-milled material was vacuum dried and then calcined in a muffle furnace at a heating rate of 3 ° C / min, a calcination temperature of 1150 ° C, and a time of 6 h to obtain 1.25Ba2Mg 2.5 Fe 11.5 O 22 ·3BaTiO3 oxide composite material.

[0094] Example 4

[0095] The difference between this embodiment and embodiment 1 is that the chemical formula of the ferrite composite material provided in this embodiment is 1.5Ba2Mg2Fe 12 O 22 ·3BaTiO3, accordingly, in the preparation method provided in this embodiment, Ba2Mg2Fe 12 O 22 The molar ratio of the pre-sintered material to the BaTiO3 pre-sintered material is 1.5:3. The rest of the contents are the same as those in Example 1.

[0096] The magnetic permeability spectrum of the ferrite composite material provided in this embodiment is as follows Figure 2 As can be seen from the figure, 1.5Ba2Mg2Fe 12 O22 ·3BaTiO3 ferrite composite material has higher initial permeability, narrower natural resonance linewidth and lower imaginary part of permeability.

[0097] Example 5

[0098] The difference between this embodiment and embodiment 1 is that the chemical formula of the ferrite composite material provided in this embodiment is 2Ba2Mg2Fe 12 O 22 ·3BaTiO3, accordingly, in the preparation method provided in this embodiment, Ba2Mg2Fe 12 O 22 The molar ratio of the pre-sintered material to the BaTiO3 pre-sintered material is 2:3. The rest of the contents are the same as those in Example 1.

[0099] The magnetic permeability spectrum of the ferrite composite material provided in this embodiment is as follows Figure 3 As can be seen from the figure, 2Ba2Mg2Fe 12 O 22 ·3BaTiO3 material has a high initial permeability but the natural resonance frequency is too low, resulting in a slightly low Snoek product.

[0100] Example 6

[0101] The difference between this embodiment and embodiment 1 is that the 1.25Ba2Mg2Fe 12 O 22 In the preparation method of the 3BaTiO3 ferrite composite material, the calcination temperature of 1200° C. in step (2) is replaced by 1100° C. The rest of the contents are the same as those in Example 1.

[0102] Example 7

[0103] The difference between this embodiment and embodiment 1 is that the 1.25Ba2Mg2Fe 12 O 22 In the preparation method of the 3BaTiO3 ferrite composite material, the calcination temperature of 1200° C. in step (2) is replaced by 1300° C. The rest of the contents are the same as those in Example 1.

[0104] Performance Test:

[0105] The magnetic permeability spectra of the ferrite composite materials provided in the above Examples 1-7 were tested at 100 MHz-18 GHz using a vector network measuring instrument, and the damping coefficient α was obtained by fitting.

[0106] Table 1 shows the performance results of the natural resonance frequency, initial magnetic permeability, Snoek product and damping coefficient α of the ferrite composite materials provided in Examples 1-7, wherein Snoek product = μ′×fr .

[0107] Table 1

[0108]

[0109] Table 2 shows the magnetic permeability (μ), dielectric constant (δ), dielectric loss tangent tan δ and magnetic loss tan δ / μ of the ferrite composite materials provided by Examples 1-7 at 1 GHz to 3 GHz.

[0110] Table 2

[0111]

[0112] From the test results in Table 1 and Table 2, we can see that:

[0113] (1) It can be seen from Examples 1 to 5 that the present invention provides a ferrite material (Ba2Mg a Fe b O 22 ) and barium titanate (BaTiO3) in different proportions, the crystal structure of the original Y-type ferrite was changed, and by adjusting the value of x in the chemical formula of the ferrite composite material, the natural resonance frequency, initial magnetic permeability and magnetic loss of the ferrite material were controlled and regulated, so that the ferrite composite material has the advantages of higher Snoek product and lower magnetic loss.

[0114] Furthermore, it can be seen from Examples 1, 4 and 5 that the present invention can further improve the Snoek product of the ferrite composite material and further reduce the damping coefficient and magnetic loss of the material by further regulating the value range of x.

[0115] pass Figure 1-3 It can be seen that changing the ratio between ferrite material and barium titanate can control the initial magnetic permeability and natural resonance frequency of the material, and thus play a role in different frequency bands and different needs.

[0116] (2) By comparing Example 1 with Examples 6-7, it can be seen that if Ba2Mg a Fe b O 22 If the temperature of the co-sintering of the pre-sintered material and the BaTiO3 pre-sintered material is too low, the reaction will be incomplete and unreacted Y-type ferrite phase will still exist, which will fail to effectively reduce the damping coefficient of the ferrite composite material and increase the initial magnetic permeability of the composite material; if the temperature is too high, impure phases will be generated, reducing the initial magnetic permeability, resulting in a higher damping coefficient of the final ferrite composite material, affecting the magnetic properties of the product.

[0117] In summary, the present invention provides a ferrite material (Ba2Mg a Fe b O 22 ) and barium titanate (BaTiO3) in different proportions, the crystal structure of the original Y-type ferrite was changed, and by adjusting the value of x in the chemical formula of the ferrite composite material, the natural resonance frequency, initial magnetic permeability and magnetic loss of the ferrite material were controlled and regulated, so that the ferrite composite material has the advantages of higher Snoek product and lower magnetic loss.

[0118] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A ferrite composite material, characterized in that: The chemical formula of the ferrite composite material is xBa2Mg a Fe b O 22 3BaTiO3, wherein a is 1.5-2.5, b is 11.5-12.5, and x is 1.1-2.

0.

2. The ferrite composite material according to claim 1, characterized in that: The chemical formula of the ferrite composite material is xBa2Mg a Fe b O 22 3BaTiO3, wherein a is 1.5-2.5, b is 11.5-12.5, and x is 1.1-1.5; Preferably, the particle size D50 of the ferrite composite material is 0.5-5 μm; Preferably, the initial magnetic permeability of the ferrite composite material is 1.5-11.8; Preferably, the damping coefficient of the ferrite composite material is 0.1-0.

73.

3. A method for preparing a ferrite composite material according to claim 1 or 2, characterized in that: The preparation method comprises: (1) A first barium source, a magnesium source and an iron source are first mixed and calcined to obtain Ba2Mg a Fe b O 22 Pre-burned material, where a is 1.5-2.5 and b is 11.5-12.5; (2) The Ba2Mg a Fe b O 22 The pre-sintered material and BaTiO3 are mixed for a second time at a molar ratio of (1.1-2.0):3, and after a second calcination, the ferrite composite material is obtained.

4. The preparation method according to claim 3, characterized in that: The preparation method of BaTiO3 comprises: The second barium source and the titanium source are mixed for a third time, and after a third calcination, the BaTiO3 is obtained; Preferably, the first barium source and the second barium source independently include BaCO3 and / or BaO; Preferably, the titanium source comprises TiO2; Preferably, the magnesium source comprises MgO and / or MgCO3; Preferably, the iron source includes any one of Fe2O3, Fe2(CO)3 or Fe(CH3COO)3, or a combination of at least two of them.

5. The preparation method according to claim 3 or 4, characterized in that: The Ba2Mg a Fe b O 22 The pre-burned material is Y-type ferrite material; Preferably, the first mixing, the second mixing and the third mixing independently include any one of ball milling, vibration milling or stirring, preferably ball milling.

6. The preparation method according to any one of claims 3 to 5, characterized in that: The first mixing speed is 600-1500rad / min; Preferably, the first mixing time is 2-4h; Preferably, a first solvent is also added during the first mixing process; Preferably, the first mixed material is further dried; Preferably, the heating rate of the first calcination is 2-3°C / min; Preferably, the temperature of the first calcination is 1100-1200°C; Preferably, the first calcination time is 3-5 hours.

7. The preparation method according to any one of claims 3 to 6, characterized in that: The second mixing speed is 600-1500rad / min; Preferably, the second mixing time is 2-4h; Preferably, a second solvent is also added during the second mixing process; Preferably, the particle size D50 of the material obtained after the second mixing is 0.5-2 μm; Preferably, the second mixed material is further dried; Preferably, the heating rate of the second calcination is 2-3°C / min; Preferably, the temperature of the second calcination is 1150-1250°C; Preferably, the second calcination time is 1-6 hours.

8. The preparation method according to any one of claims 4 to 7, characterized in that: The rotation speed of the third mixing is 600-1500rad / min; Preferably, the third mixing time is 2-4h; Preferably, a third solvent is also added during the third mixing process; Preferably, the third mixed material is further dried; Preferably, the heating rate of the third calcination is 2-3°C / min; Preferably, the temperature of the third calcination is 1000-1250°C; Preferably, the third calcination time is 3-5 hours.

9. The preparation method according to any one of claims 3 to 8, characterized in that: The preparation method comprises: (1) mixing a first barium source, a magnesium source, an iron source and a first solvent for 2-4 hours at a mixing speed of 600-1500 rad / min, drying the mixed material, and then calcining it at 1100-1200° C. for 3-5 hours at a heating rate of 2-3° C. / min to obtain Ba2Mg a Fe b O 22 Pre-sintered material; wherein a is 1.5-2.5, b is 11.5-12.5, and the obtained Ba2Mg a Fe b O 22 The pre-burned material is Y-type ferrite material; The second barium source, the titanium source and the third solvent are mixed for 2-4 hours at a mixing speed of 600-1500 rad / min, the mixed material is dried, and then calcined at 1000-1250° C. for 3-5 hours at a calcination heating rate of 2-3° C. / min to obtain a BaTiO3 pre-sintered material; (2) The Ba2Mg a Fe b O 22 The pre-sintered material, the BaTiO3 pre-sintered material and the second solvent are mixed for 2-4 hours, wherein Ba2Mg a Fe b O 22 The molar ratio of the pre-sintered material and the BaTiO3 pre-sintered material is (1.1-2.0):3, the mixing speed is 600-1500rad / min, the particle size D50 of the mixed material is 0.5-2μm, the mixed material is dried, and then calcined at 1150-1250℃ for 1-6h, and the calcination heating rate is 2-3℃ / min to obtain the ferrite composite material.