Design method of energy-saving kiln
By adjusting the kiln structure and selecting high-efficiency bricks, the problems of high energy consumption and low glass liquid quality are solved, and energy consumption and glass quality are reduced to meet the needs of high-end customers.
Patent Information
- Application Number
- CN202411180681.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-12-03
AI Technical Summary
The existing glass production kilns have high energy consumption and low glass liquid quality, resulting in high production costs, low yield and unstable glass rib defects, which cannot meet the needs of high-end customers.
Design an energy-saving kiln. By adjusting the pool depth, paving brick thickness and heat storage chamber design in each area of the kiln, high-efficiency bricks such as AZS-41VF and P-D energy-saving silicon bricks are selected to improve the structure of the kiln to reduce energy consumption and improve glass quality.
It has achieved a reduction in energy consumption by 11% and a reduction in glass defect density by 75%, improving glass quality and meeting the needs of high-end customers.
Smart Images

Figure CN119059719A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass production equipment, and in particular relates to a design method for an energy-saving kiln. Background Art
[0002] The kiln is the most important thermal equipment in a glass factory. Its function is to melt, clarify and homogenize the mixed raw materials to provide high-quality and qualified glass liquid for the next process. At present, the kilns of glass production enterprises have the problems of high energy consumption and low quality of glass liquid. On the one hand, it causes high production costs for enterprises; on the other hand, there are too many point defects in the glass, with an average of 10m 2 Glass has more than two defects, resulting in low product yield and low yield. In addition, the glass rib defects are unstable and cannot meet the needs of high-end customers. Summary of the invention
[0003] The purpose of the present invention is to provide a design method for an energy-saving kiln, which effectively solves the problems of high energy consumption and low quality of glass liquid in current kilns.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is:
[0005] A design method for an energy-saving kiln, wherein the kiln is composed of a melting area, a clarification area, a neck, a working part, a small furnace, a heat storage chamber and a flue.
[0006] The pool depth of the melting zone is 1350mm, the thickness of the paving bricks in the melting zone is 100mm, and the pool wall bricks in the melting zone are AZS-41VF model.
[0007] The pool depth of the clarification area is 1134mm. The paving bricks in the clarification area are laid in two layers and the thickness of each layer of paving bricks is 75mm. The pool wall bricks in the clarification area are of AZS-36ENC model.
[0008] The pool depths of the neck and the working part are both 1000mm, the paving brick thickness of the working part is 100mm, and 50mm thick ramming material is set under the paving bricks of the melting area, clarification area and working part.
[0009] The heat storage chamber is divided into multiple chambers by a fully connected design. The front wall structure of the kiln is L-shaped, and the large arch bricks of the kiln are made of PD energy-saving silica bricks.
[0010] Compared with the prior art, the beneficial technical effects of the present invention are:
[0011] The present invention is conducive to reducing the energy consumption of the kiln and improving the quality of glass by designing the depth of each area of the kiln, the thickness of the paving bricks and the heat storage chamber, as well as the selection of brick materials. The kiln after cold repair by the method of the present invention has a glass defect density reduced by 75% year-on-year, and an average glass unit consumption reduced by 11% year-on-year. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a glass defect density curve diagram before and after the cold repair of the kiln in Example 1.
[0013] Figure 2 It is a glass consumption curve diagram before and after the cold repair of the kiln in Example 1. DETAILED DESCRIPTION
[0014] Embodiment 1: This embodiment takes the glass kiln of Q factory as an example to explain the technical scheme of the present invention in detail.
[0015] The glass kiln of Q Factory consists of a melting zone (also called a flame zone), a clarification zone, a neck, a working part, a small furnace, a heat storage chamber and a flue. Before the cold repair using the design method of the energy-saving kiln of the present invention, the pool depths of the melting zone, clarification zone, neck and working part are all 1143mm; the thickness of the paving bricks of the melting zone, clarification zone and working part is 75mm; only the paving bricks of the melting zone and clarification zone are provided with ramming materials under them; there are 6 heat storage chambers, and the 6 heat storage chambers are fully connected; the front wall structure of the kiln is J-shaped. In terms of brick materials, before the cold repair: the pool wall bricks of the melting zone are selected from the AZS-36ENC model, the pool wall bricks of the clarification zone are selected from the AZS-33RC model, and the large arch bricks of the kiln are made of domestic high-quality silica bricks.
[0016] After cold repair using the design method of the energy-saving kiln of the present invention, the pool depth in the melting zone is 1350 mm, the pool depth in the clarification zone is 1134 mm, and the pool depths in the neck and working parts are both 1000 mm, which is beneficial to energy saving, improving glass quality and reducing high temperature erosion of the pool bottom.
[0017] After cold repair, the thickness of the paving bricks in the melting zone is 100mm, the paving bricks in the clarification zone are laid in two layers and the thickness of each layer of paving bricks is 75mm, and the thickness of the paving bricks in the working part is 100mm, which is beneficial to increase the erosion resistance of the pool bottom.
[0018] After cold repair, not only are ramming materials placed under the paving bricks in the melting and clarification zones, but 50mm thick ramming materials are also added under the paving bricks in the working section, thereby increasing the anti-erosion capacity of the pool bottom and having the effect of heat preservation and energy saving. The front wall structure of the kiln is designed to be L-shaped, which is conducive to increasing the coverage area of the feeding pool, improving the pre-melting effect of the mixed material, and reducing dust.
[0019] After the cold repair, the six regenerators were changed from fully connected to 2-2-2 separation, that is, the six regenerators were separated in pairs, so that the combustion effect of each small furnace could be better controlled. If the combustion effect is considered alone, it is best to separate the six regenerators separately (i.e. 1-1-1-1-1-1 separation), but this separation method has too many partition walls, which reduces the heat exchange area of the regenerator, thereby affecting the thermal efficiency. The applicant comprehensively considered the control of the heat exchange area (thermal efficiency) and the combustion effect and adopted the 2-2-2 separation method.
[0020] In terms of brick materials, after cold repair, the pool wall bricks in the melting area are AZS-41VF model, and the pool wall bricks in the clarification area are AZS-36ENC model, which is conducive to improving the wear resistance and erosion resistance of the pool wall bricks. The large arch bricks of the kiln are PD energy-saving silica bricks imported from Germany, which is conducive to increasing the radiation area and improving the thermal radiation rate.
[0021] The comparison results of glass quality and energy consumption of the glass furnace in Q factory before and after cold repair by adopting the design method of the energy-saving furnace of the present invention are as follows: Figure 1 and Figure 2 As shown, the average defect density of the glass before cold repair is 2.17pc / 10m 2 After cold repair, the density of glass defects is 0.55pc / 10m 2 , down 75% year-on-year. The average glass unit consumption before cold repair was 1648kcal / kg·g, and the average glass unit consumption after cold repair was 1468kcal / kg·g, down 11% year-on-year. Therefore, using the method of the present invention to repair the kiln after cold repair is conducive to reducing energy consumption and improving glass quality.
[0022] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by technicians in this technical field within the essential scope of the present invention should also fall within the protection scope of the present invention.
Claims
1. A design method for energy-saving kiln, It is characterized in that The kiln is composed of a melting area, a clarification area, a neck, a working part, a small furnace, a regenerator and a flue; The pool depth of the melting zone is 1350mm, the thickness of the paving bricks in the melting zone is 100mm, and the pool wall bricks in the melting zone are AZS-41VF model; The pool depth of the clarification area is 1134mm. The paving bricks in the clarification area are laid in two layers and the thickness of each layer of paving bricks is 75mm. The pool wall bricks in the clarification area are AZS-36ENC model; The depth of the tank for the neck and the working part is 1000mm, the thickness of the paving bricks for the working part is 100mm, and 50mm thick ramming material is set under the paving bricks of the melting area, clarification area and working part; The heat storage chamber is divided into multiple chambers, the front wall structure of the kiln is L-shaped, and the large arch bricks of the kiln are made of PD energy-saving silica bricks.
Citation Information
Patent Citations
Glass kiln feeding port device
CN107721133A
Stepped furnace tank of plate glass transverse flame melting furnace
CN112919775A
Floating-method glass smelting kiln related to production of ultrathin glass
CN203200155U
Temperature adjusting device for cooling part of glass kiln
CN221522391U
Melting chamber of bath glass-making furnace
SU1342881A1