High-temperature-resistant quartz roller for glass tempering furnace and preparation method of high-temperature-resistant quartz roller

By forming a composite coating of inorganic oxide and basalt fibers on the surface of the quartz roller, the problem of crystallization of quartz rollers at high temperatures is solved, the high temperature resistance and strength are improved, and the surface quality during the fiberglass tempering process is improved.

CN119059730AActive Publication Date: 2024-12-03BEIHAI LONGHAO PHOTOELECTRIC TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411181574.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

In the fiberglass tempering furnace, the quartz rollers are prone to crystallization at high temperatures, resulting in defects and defects on the glass surface. The existing quartz rollers have defects when used at high temperatures.

Method used

A high-temperature resistant coating formed by composite of inorganic oxide and basalt fibers is formed on the surface of the quartz roller. The high-temperature resistant and strength of the coating is improved through the interlocking network structure of aluminum oxide, silica powder and basalt fibers.

Benefits of technology

It effectively improves the high temperature resistance and strength of quartz rollers, reduces dimensional deformation at high temperatures, and improves the surface quality during the fiberglass tempering process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012318380000091
    Figure BDA0005012318380000091
  • Figure BDA0005012318380000101
    Figure BDA0005012318380000101
Patent Text Reader

Abstract

The invention provides a high-temperature-resistant quartz roller for a glass tempering furnace and a preparation method of the high-temperature-resistant quartz roller. The high-temperature-resistant quartz roller comprises a quartz roller body and a high-temperature-resistant coating, wherein the surface of the quartz roller body is coated with the high-temperature-resistant coating; the high-temperature-resistant coating comprises the following components in parts by weight: 100 parts of alumina powder, 20-40 parts of silicon oxide powder, 15-25 parts of basalt fibers and 3-7 parts of a binder. According to the high-temperature-resistant quartz roller for the glass tempering furnace and the preparation method of the high-temperature-resistant quartz roller, the high-temperature-resistant coating formed by compounding the inorganic oxide and the basalt fiber is formed on the surface of the quartz roller, so that the quartz roller has the advantages of high strength and small high-temperature deformation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass tempering production, and in particular to a high temperature resistant quartz roller for a glass tempering furnace and a preparation method thereof. Background Art

[0002] Glass tempering furnace is an industrial heating equipment. Glass is transported and heated by quartz rollers in the tempering furnace. Therefore, the principle of tempering glass is that the glass needs to be heated to near the melting point in the furnace and then rapidly cooled to meet the stress requirements of the tempered glass itself. However, since the glass is in direct contact with the quartz rollers during the heating process in the tempering furnace, and the surface of the quartz rollers will continuously overflow at a high temperature of more than 650°C, it is easy to cause defects and defects on the surface of the tempered glass.

[0003] Basalt fiber has excellent mechanical properties, high chemical resistance, and can be used in a wide temperature range. These excellent properties make it possible to become a high-performance material. Therefore, if basalt fiber is used to reinforce quartz rollers, it is expected to improve the defect that quartz rollers cannot be used at high temperatures. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a high-temperature resistant quartz roller for a glass tempering furnace and a preparation method thereof. By forming a high-temperature resistant coating composed of an inorganic oxide and basalt fiber on the surface of the quartz roller, the quartz roller has the advantages of high strength and small high-temperature deformation.

[0005] The present invention provides a high temperature resistant quartz roller for a glass tempering furnace, comprising a quartz roller body and a high temperature resistant coating covering the surface of the quartz roller body;

[0006] The high temperature resistant coating comprises, by weight: 100 parts of aluminum oxide powder, 20-40 parts of silicon oxide powder, 15-25 parts of basalt fiber, and 3-7 parts of a binder.

[0007] In the present invention, a high-temperature resistant coating is formed on the surface of the quartz roller body. The high-temperature resistant coating is based on an inorganic oxide powder containing aluminum oxide and silicon oxide, and basalt fiber is additionally added. When sintered at high temperature, an interlocking network structure can be formed between the basalt fiber and the inorganic oxide powder, ensuring that the coating still maintains good dimensional stability under high temperature conditions, and its high temperature resistance and strength properties are guaranteed.

[0008] Preferably, the quartz roller body is prepared by sintering quartz sand with a purity higher than 99.9%.

[0009] Preferably, the alumina powder has a particle size of 0.5-10 μm and a purity higher than 99.9%.

[0010] Preferably, the silicon oxide powder has a particle size of 0.5-10 μm and a purity higher than 99.9%.

[0011] Preferably, the basalt fiber is a silica-coated basalt fiber;

[0012] Preferably, the silicon oxide coated basalt fiber is formed by grafting an aminosilane coupling agent onto the surface of the basalt fiber and then mixing and curing the basalt fiber with silica sol.

[0013] In the present invention, by first grafting an aminosilane coupling agent on the surface of the basalt fiber, the surface of the basalt fiber has an amino group. When it is mixed with silica sol, the amino group can first react with the silanol group of the silica sol, thereby allowing the silica gel to firmly adhere to the surface of the basalt fiber, which not only improves the adhesion effect between the silica gel and the basalt fiber, but also can effectively coat the surface of the basalt fiber with silica after curing, thereby further improving the temperature resistance of the basalt fiber, and can increase the wetting and entanglement effect of the basalt fiber with the inorganic oxide powders of alumina and silica, and further improve the temperature resistance and strength performance of the obtained coating.

[0014] Preferably, the length of the basalt fiber is 10-100 μm, and the aspect ratio is 5-10; the aminosilane coupling agent is 3-aminopropyltrimethoxysilane or 3-(2-aminoethylamino)propyltrimethoxysilane; and the content of silicon oxide in the silica sol is 20-25 wt%.

[0015] Preferably, the binder is polyamic acid;

[0016] Preferably, the polyamic acid is formed by polycondensing a rigid dibasic acid anhydride and a flexible diamine;

[0017] Preferably, the rigid dibasic acid anhydride is at least one of pyromellitic anhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride or 3,3',4,4'-benzophenonetetracarboxylic anhydride, and the flexible diamine is at least one of 1,3-bis(4'-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 4,4'-diaminodiphenyl ether or 2,2-bis[4-(4-aminophenoxy)phenyl]propane.

[0018] In the present invention, polyamic acid is used as a binder, and its polyimide segment can provide extremely excellent high temperature resistance. It can still act as a binder during high temperature sintering, promoting the effective formation of a high temperature resistant coating to obtain better thermal stability and high temperature resistance.

[0019] The present invention also provides a method for preparing a high temperature resistant quartz roller for a glass tempering furnace, comprising the following steps:

[0020] S1. Provide a quartz roller body;

[0021] S2, mixing 100 parts of alumina powder, 20-40 parts of silicon oxide powder, 15-25 parts of basalt fiber, 3-7 parts of a binder and 4-10 parts of water by weight, and ball milling to obtain a mixed slurry;

[0022] S3, coating the mixed slurry on the surface of the quartz roller body, drying, and sintering to obtain the high temperature resistant quartz roller for the glass tempering furnace.

[0023] Preferably, the ball milling rate is 50-200 rpm, and the ball milling time is 6-12 h.

[0024] Preferably, the drying temperature is 60-80°C and the drying time is 5-10h;

[0025] Preferably, the sintering comprises: heating to 500-600°C at a rate of 1-3°C / min and then keeping the temperature for 1-3h, and then heating to 1200-1300°C at a rate of 2-4°C / min and then keeping the temperature for 3-5h.

[0026] The present invention provides a high temperature resistant quartz roller for a glass tempering furnace and a preparation method thereof, wherein a layer of high temperature resistant coating is formed on the surface of a conventional quartz roller body, thereby protecting the quartz roller body and improving the high temperature resistance and strength performance of the quartz roller. DETAILED DESCRIPTION

[0027] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0028] Example 1

[0029] A high temperature resistant quartz roller for a glass tempering furnace, the preparation method of which comprises:

[0030] (1) high-purity quartz sand (purity higher than 99.9% and average particle size D50 of 15 μm) is slurry-casted to obtain a quartz roller body;

[0031] (2) 100 parts of alumina powder (purity higher than 99.9%, average particle size D50 of 5 μm), 30 parts of silicon oxide powder (purity higher than 99.9%, average particle size D50 of 5 μm), 20 parts of basalt fiber (average length of 30 μm, average aspect ratio of 3), 25 parts of polyamic acid solution and 12 parts of deionized water were mixed by weight, added to a ball mill and ball milled for 8 h, using zirconium oxide balls as ball milling media during ball milling, and the ball milling speed was 100 rpm to obtain a mixed slurry;

[0032] The polyamic acid solution is prepared by the following method: adding 1,3-bis(4'-aminophenoxy)benzene and pyromellitic dianhydride in a molar ratio of 1:1 into N-methylpyrrolidone (NMP), stirring and dissolving them completely, and stirring and reacting for 4 hours under nitrogen protection to obtain a polyamic acid solution with a content of 20wt%;

[0033] (3) The mixed slurry is coated on the surface of the quartz roller body, and dried naturally at room temperature and in the shade for 12 hours, and then dried at 60°C for 8 hours, and then heated to 550°C at a rate of 2°C / min and kept warm for 2 hours, and then heated to 1250°C at a rate of 3°C / min and kept warm for 4 hours, and naturally cooled to obtain a high-temperature resistant quartz roller for a glass tempering furnace.

[0034] Example 2

[0035] A high temperature resistant quartz roller for a glass tempering furnace, the preparation method of which comprises:

[0036] (1) high-purity quartz sand (purity higher than 99.9% and average particle size D50 of 15 μm) is slurry-casted to obtain a quartz roller body;

[0037] (2) 100 parts of alumina powder (purity higher than 99.9%, average particle size D50 of 5 μm), 20 parts of silicon oxide powder (purity higher than 99.9%, average particle size D50 of 5 μm), 25 parts of basalt fiber (average length of 30 μm, average aspect ratio of 3), 15 parts of polyamic acid solution and 15 parts of deionized water were mixed by weight, and the mixture was added to a ball mill and ball milled for 12 h. Zirconia balls were used as ball milling media during ball milling, and the ball milling speed was 50 rpm to obtain a mixed slurry;

[0038] The polyamic acid solution is prepared by the following method: adding 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane and 1,4,5,8-naphthalenetetracarboxylic anhydride in a molar ratio of 1:1 into N-methylpyrrolidone (NMP), stirring and dissolving them completely, stirring and reacting for 4 hours under nitrogen protection, to obtain a polyamic acid solution with a content of 20wt%;

[0039] (3) The mixed slurry is coated on the surface of the quartz roller body, and dried naturally at room temperature and in the shade for 12 hours, and then dried at 80°C for 5 hours, and then heated to 600°C at a rate of 1°C / min and kept warm for 1 hour, and then heated to 1200°C at a rate of 4°C / min and kept warm for 5 hours, and naturally cooled to obtain a high-temperature resistant quartz roller for a glass tempering furnace.

[0040] Example 3

[0041] A high temperature resistant quartz roller for a glass tempering furnace, the preparation method of which comprises:

[0042] (1) high-purity quartz sand (purity higher than 99.9% and average particle size D50 of 15 μm) is slurry-casted to obtain a quartz roller body;

[0043] (2) 100 parts of alumina powder (purity higher than 99.9%, average particle size D50 of 5 μm), 40 parts of silicon oxide powder (purity higher than 99.9%, average particle size D50 of 5 μm), 15 parts of basalt fiber (average length of 30 μm, average aspect ratio of 3), 35 parts of polyamic acid solution and 5 parts of deionized water were mixed by weight, added to a ball mill and ball milled for 6 hours, using zirconium oxide balls as ball milling media during ball milling, and the ball milling speed was 200 rpm to obtain a mixed slurry;

[0044] The polyamic acid solution is prepared by the following method: adding 4,4'-diaminodiphenyl ether and 3,3',4,4'-biphenyltetracarboxylic dianhydride in a molar ratio of 1:1 into N-methylpyrrolidone (NMP), stirring and dissolving them completely, stirring and reacting for 4 hours under nitrogen protection, to obtain a polyamic acid solution with a content of 20wt%;

[0045] (3) The mixed slurry is coated on the surface of the quartz roller body, and dried naturally at room temperature and in the shade for 12 hours, and then dried at 70°C for 10 hours, and then heated to 500°C at a rate of 3°C / min and kept warm for 3 hours, and then heated to 1300°C at a rate of 2°C / min and kept warm for 3 hours, and naturally cooled to obtain a high-temperature resistant quartz roller for a glass tempering furnace.

[0046] Example 4

[0047] A high temperature resistant quartz roller for a glass tempering furnace, the preparation method of which comprises:

[0048] (1) high-purity quartz sand (purity higher than 99.9% and average particle size D50 of 15 μm) is slurry-casted to obtain a quartz roller body;

[0049] (2) 100 parts of alumina powder (purity higher than 99.9%, average particle size D50 of 5 μm), 30 parts of silica powder (purity higher than 99.9%, average particle size D50 of 5 μm), 20 parts of silica-coated basalt fiber, 25 parts of polyamic acid solution and 12 parts of deionized water were mixed by weight, and the mixture was added to a ball mill for 8 h, using zirconium oxide balls as the ball milling medium, and the ball milling speed was 100 rpm to obtain a mixed slurry;

[0050] The silicon oxide coated basalt fiber is prepared by the following method: adding basalt fiber (average length of 30 μm, average aspect ratio of 3) to an acetic acid solution (acetic acid content of 0.05 wt%) containing 0.5 wt% of 3-aminopropyltrimethoxysilane, ultrasonically reacting at 60° C. for 2 h, filtering, and drying to obtain basalt fiber with surface grafted aminosilane coupling agent; adding tetraethyl orthosilicate to anhydrous ethanol to dissolve completely, then adding nitric acid aqueous solution, the amount of nitric acid used is 1 times the molar amount of tetraethyl orthosilicate, heating to 40° C. and stirring for reaction for 2 h to obtain silica sol with a silicon oxide content of 25 wt%; adding the basalt fiber with surface grafted aminosilane coupling agent to the silica sol and mixing, the mass ratio of basalt fiber to silica sol is 1:0.6, drying, and curing at 200° C. for 24 h to obtain silicon oxide coated basalt fiber;

[0051] The polyamic acid solution is prepared by the following method: adding 1,3-bis(4'-aminophenoxy)benzene and pyromellitic dianhydride in a molar ratio of 1:1 into N-methylpyrrolidone (NMP), stirring and dissolving them completely, and stirring and reacting for 4 hours under nitrogen protection to obtain a polyamic acid solution with a content of 20wt%;

[0052] (3) The mixed slurry is coated on the surface of the quartz roller body, and dried naturally at room temperature and in the shade for 12 hours, and then dried at 60°C for 8 hours, and then heated to 550°C at a rate of 2°C / min and kept warm for 2 hours, and then heated to 1250°C at a rate of 3°C / min and kept warm for 4 hours, and naturally cooled to obtain a high-temperature resistant quartz roller for a glass tempering furnace.

[0053] Comparative Example 1

[0054] A high temperature resistant quartz roller for a glass tempering furnace, the preparation method of which comprises:

[0055] (1) high-purity quartz sand (purity higher than 99.9% and average particle size D50 of 15 μm) is slurry-casted to obtain a quartz roller body;

[0056] (2) 100 parts of aluminum oxide powder (purity higher than 99.9%, average particle size D50 of 5 μm), 30 parts of silicon oxide powder (purity higher than 99.9%, average particle size D50 of 5 μm), 25 parts of polyamic acid solution and 12 parts of deionized water were mixed by weight, and the mixture was added to a ball mill for 8 hours, using zirconium oxide balls as the ball milling medium at a ball milling rate of 100 rpm to obtain a mixed slurry;

[0057] The polyamic acid solution is prepared by the following method: adding 1,3-bis(4'-aminophenoxy)benzene and pyromellitic dianhydride in a molar ratio of 1:1 into N-methylpyrrolidone (NMP), stirring and dissolving them completely, and stirring and reacting for 4 hours under nitrogen protection to obtain a polyamic acid solution with a content of 20wt%;

[0058] (3) The mixed slurry is coated on the surface of the quartz roller body, and dried naturally at room temperature and in the shade for 12 hours, and then dried at 60°C for 8 hours, and then heated to 550°C at a rate of 2°C / min and kept warm for 2 hours, and then heated to 1250°C at a rate of 3°C / min and kept warm for 4 hours, and naturally cooled to obtain a high-temperature resistant quartz roller for a glass tempering furnace.

[0059] Comparative Example 2

[0060] A high temperature resistant quartz roller for a glass tempering furnace, the preparation method of which comprises:

[0061] (1) high-purity quartz sand (purity higher than 99.9% and average particle size D50 of 15 μm) is slurry-casted to obtain a quartz roller body;

[0062] (2) 100 parts of alumina powder (purity higher than 99.9%, average particle size D50 of 5 μm), 30 parts of silicon oxide powder (purity higher than 99.9%, average particle size D50 of 5 μm), 20 parts of basalt fiber (average length of 30 μm, average aspect ratio of 3), 5 parts of carboxymethyl cellulose fiber and 12 parts of deionized water were mixed by weight, and the mixture was added to a ball mill for 8 h, using zirconium oxide balls as the ball milling medium, and the ball milling speed was 100 rpm to obtain a mixed slurry;

[0063] (3) The mixed slurry is coated on the surface of the quartz roller body, and dried naturally at room temperature and in the shade for 12 hours, and then dried at 60°C for 8 hours, and then heated to 550°C at a rate of 2°C / min and kept warm for 2 hours, and then heated to 1250°C at a rate of 3°C / min and kept warm for 4 hours, and naturally cooled to obtain a high-temperature resistant quartz roller for a glass tempering furnace.

[0064] Comparative Example 3

[0065] A high temperature resistant quartz roller for a glass tempering furnace, the preparation method of which comprises:

[0066] (1) high-purity quartz sand (purity higher than 99.9% and average particle size D50 of 15 μm) is slurry-casted to obtain a quartz roller body;

[0067] (2) 100 parts of alumina powder (purity higher than 99.9%, average particle size D50 of 5 μm), 30 parts of silica powder (purity higher than 99.9%, average particle size D50 of 5 μm), 20 parts of silica-coated basalt fiber, 25 parts of polyamic acid solution and 12 parts of deionized water were mixed by weight, and the mixture was added to a ball mill for 8 h, using zirconium oxide balls as the ball milling medium, and the ball milling speed was 100 rpm to obtain a mixed slurry;

[0068] The silicon oxide coated basalt fiber is prepared by the following method: adding tetraethyl orthosilicate to anhydrous ethanol and dissolving it completely, then adding nitric acid aqueous solution, the amount of nitric acid used is 1 times the molar amount of tetraethyl orthosilicate, heating to 40° C. and stirring for reaction for 2 hours to obtain a silica sol with a silicon oxide content of 25wt%; adding basalt fiber (average length of 30 μm, average aspect ratio of 3) to the silica sol and mixing, the mass ratio of basalt fiber to silica sol is 1:0.6, drying, and curing at 200° C. for 24 hours to obtain a silicon oxide coated basalt fiber;

[0069] The polyamic acid solution is prepared by the following method: adding 1,3-bis(4'-aminophenoxy)benzene and pyromellitic dianhydride in a molar ratio of 1:1 into N-methylpyrrolidone (NMP), stirring and dissolving them completely, and stirring and reacting for 4 hours under nitrogen protection to obtain a polyamic acid solution with a content of 20wt%;

[0070] (3) The mixed slurry is coated on the surface of the quartz roller body, and dried naturally at room temperature and in the shade for 12 hours, and then dried at 60°C for 8 hours, and then heated to 550°C at a rate of 2°C / min and kept warm for 2 hours, and then heated to 1250°C at a rate of 3°C / min and kept warm for 4 hours, and naturally cooled to obtain a high-temperature resistant quartz roller for a glass tempering furnace.

[0071] The compressive strength of the high temperature resistant quartz rollers obtained in the examples and comparative examples was tested according to the standard GB / T4740-1999, and the bending strength was tested according to the standard GB / T 4741-1999. The specific results are shown in Table 1 below:

[0072] Table 1 Performance results of the high temperature resistant quartz rollers described in the examples and comparative examples

[0073]

[0074]

[0075] It can be seen from the above table that the quartz roller described in the embodiment has the advantages of high strength and small high-temperature deformation. In contrast, the performance of the quartz roller in the comparative example is inferior; and it can be seen from comparative example 3 that even if the basalt fiber is coated with silicon oxide, if it is not modified in advance with an aminosilane coupling agent, the performance improvement effect of the silicon oxide-coated basalt fiber on the quartz roller relative to the uncoated basalt fiber is also very limited. This may be because if the aminosilane coupling agent is not used in advance for modification, silicon oxide cannot achieve effective coating of the basalt fiber.

[0076] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A high temperature resistant quartz roller for a glass tempering furnace, characterized in that: It comprises a quartz roller body and a high temperature resistant coating covering the surface of the quartz roller body; The high temperature resistant coating comprises, by weight: 100 parts of aluminum oxide powder, 20-40 parts of silicon oxide powder, 15-25 parts of basalt fiber, and 3-7 parts of a binder.

2. The high temperature resistant quartz roller for a glass tempering furnace according to claim 1, characterized in that: The quartz roller body is formed by sintering quartz sand with a purity higher than 99.9%.

3. The high temperature resistant quartz roller for a glass tempering furnace according to claim 1 or 2, characterized in that: The particle size of the aluminum oxide powder is 0.1-10 μm, and the purity is higher than 99.9%.

4. The high temperature resistant quartz roller for a glass tempering furnace according to any one of claims 1 to 3, characterized in that: The silicon oxide powder has a particle size of 0.1-10 μm and a purity higher than 99.9%.

5. The high temperature resistant quartz roller for a glass tempering furnace according to any one of claims 1 to 4, characterized in that: The basalt fiber is a silicon oxide coated basalt fiber; Preferably, the silicon oxide coated basalt fiber is formed by grafting an aminosilane coupling agent onto the surface of the basalt fiber and then mixing and curing the basalt fiber with silica sol.

6. The high temperature resistant quartz roller for a glass tempering furnace according to claim 5, characterized in that: The length of the basalt fiber is 10-100 μm, and the aspect ratio is 5-10; the aminosilane coupling agent is 3-aminopropyltrimethoxysilane or 3-(2-aminoethylamino)propyltrimethoxysilane; and the content of silicon oxide in the silica sol is 20-25 wt%.

7. The high temperature resistant quartz roller for a glass tempering furnace according to any one of claims 1 to 6, characterized in that: The binder is polyamic acid; Preferably, the polyamic acid is formed by polycondensing a rigid dibasic acid anhydride and a flexible diamine; Preferably, the rigid dibasic acid anhydride is at least one of pyromellitic anhydride, 1,4,5,8-naphthalenetetracarboxylic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride or 3,3',4,4'-benzophenonetetracarboxylic anhydride, and the flexible diamine is at least one of 1,3-bis(4'-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 4,4'-diaminodiphenyl ether or 2,2-bis[4-(4-aminophenoxy)phenyl]propane.

8. A method for preparing a high temperature resistant quartz roller for a glass tempering furnace, characterized in that: The steps include: S1. Provide a quartz roller body; S2, mixing 100 parts of alumina powder, 20-40 parts of silicon oxide powder, 15-25 parts of basalt fiber, 3-7 parts of binder and 6-17 parts of water by weight, and ball milling to obtain a mixed slurry; S3, coating the mixed slurry on the surface of the quartz roller body, drying, and sintering to obtain the high temperature resistant quartz roller for the glass tempering furnace.

9. The method for preparing the high temperature resistant quartz roller for glass tempering furnace according to claim 8, characterized in that: The ball milling rate is 50-200 rpm, and the ball milling time is 6-12 h.

10. The method for preparing the high temperature resistant quartz roller for glass tempering furnace according to claim 8 or 9, characterized in that: The drying temperature is 60-80°C and the drying time is 5-10h; Preferably, the sintering comprises: heating to 500-600°C at a rate of 1-3°C / min and then keeping the temperature for 1-3h, and then heating to 1200-1300°C at a rate of 2-4°C / min and then keeping the temperature for 3-5h.

Citation Information

Patent Citations

  • Novel composite coating layer and preparation method thereof

    CN105565835A

  • High-temperature-resistant material for supporting roller in furnace

    CN108863409A

  • In-situ synthesis of nanometer oxide, and applications of the nanometer oxide in polyester carbon fiber sizing agents and basalt fiber / glass fiber sizing agents

    CN110128034A

  • Self-leveling polymer cement waterproof coating and preparation method thereof

    CN116063890A

  • Binder as well as preparation method and application thereof

    CN116239988A