Carbon anode antioxidant and preparation method and application thereof
By using 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite powder, and 10% alumina powder in electrolytic aluminum production, a hard protective shell is formed, and the carbon anode in material is solved. The problem of faster consumption and skewed mouth area extends the anode life and improves the quality of liquid aluminum.
Patent Information
- Application Number
- CN202310636419.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-12-03
AI Technical Summary
During the electrolytic aluminum production process, the carbon anode is easily washed by alumina powder and electrolyte at the mouth of the material, resulting in accelerated consumption and serious skew during the shelling process, which affects the service life of the anode and the final product quality.
Carbon anode antioxidant including 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite powder, and 10% alumina powder, are used to apply it to the anode surface after stirring and mixing, forming a hard protective shell to protect it. External shock.
Effectively prevent carbon anodization, reduce consumption, extend service life, prevent the electrochemical reaction between the steel claws and the electrolyte, and improve the quality of metal aluminum liquid.
Smart Images

Figure CN119059789A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrolytic aluminum, and specifically relates to a carbon anode antioxidant and a preparation method and application thereof. Background Art
[0002] During the production of electrolytic aluminum, the steel claws, aluminum guide rods, and anode carbon blocks together form the anode guide rod group, which serves as a bridge to connect the anode and transmit current. At present, electrolytic cells mostly use the middle feeding method. The carbon anode near the alumina feeding port is easily eroded by alumina powder and flowing electrolyte. At the same time, there is a deflection phenomenon during the shelling process of the shelling hammer rod, which makes the carbon anode at the feeding port hit by the hammer rod. In this way, the carbon anode at the feeding port is consumed faster than the anodes in other parts. When the anodes of the entire electrolytic cell reach the end of their service life, the replaced anodes often have a thin body (such as Figure 1 and Figure 2 , representing before and after slimming respectively), steel claws are sometimes exposed near the feed port. Before the residual anode leaves the electrolytic cell, the steel claws have already reacted electrochemically with the electrolyte, resulting in an increase in the iron content of the final product, molten aluminum, which affects the quality of the molten aluminum and is also a damage to the reused steel claws. Summary of the invention
[0003] In view of this, the purpose of the present invention is to provide a carbon anode antioxidant and its preparation method and application. The carbon anode antioxidant provided by the present invention can form a hard protective shell on the surface of the carbon anode, which can effectively protect against external impact.
[0004] In order to achieve the above purpose, the present invention provides a carbon anode antioxidant, including 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite mineral powder, and 10% alumina powder.
[0005] Preferably, the mass concentration of the sodium silicate aqueous solution is 40-50%.
[0006] Preferably, the particle size of the fluorite mineral powder is ≤0.154 mm.
[0007] Preferably, the fluorite mineral powder is fluorite mineral powder FC-97.
[0008] Preferably, the particle size of the alumina powder is less than 150 μm.
[0009] The present invention also provides a method for preparing a carbon anode antioxidant, comprising the following steps:
[0010] The sodium silicate aqueous solution, asbestos felt, fluorite ore powder and alumina powder are mixed to obtain the carbon anode antioxidant.
[0011] Preferably, the mixing comprises: first mixing the sodium silicate aqueous solution and asbestos felt, and second mixing the obtained first mixture with fluorite ore powder and alumina powder.
[0012] Preferably, the first mixing method is stirring, the stirring speed is 170-350 rpm, and the time is 2-3 min; the second mixing method is stirring, the stirring speed is 170-350 rpm, and the time is 2-3 min.
[0013] The present invention also provides the use of the carbon anode antioxidant in preventing carbon anode oxidation, and the application method is: before electrolysis, after applying the sodium silicate aqueous solution to the carbon anode, the carbon anode antioxidant is applied.
[0014] Preferably, the thickness of the coated carbon anode antioxidant is 0.4 to 0.6 cm.
[0015] The present invention provides a carbon anode antioxidant, comprising 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite ore powder, and 10% alumina powder. The glass water of the present invention is mixed with other substances and sintered at high temperature to form a hard protective shell, and the asbestos silk maintains its original physical properties after being heated, and warp and weft reinforcement ribs are formed in the hard protective shell to improve the strength of the protective shell. Therefore, when the carbon anode antioxidant provided by the present invention is used for the carbon anode, a hard protective shell can be formed on the surface of the carbon anode, which can effectively protect against external impact (shell hammer rod impact capacity), and play a role in protecting the carbon anode and steel claws. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 and Figure 2 The actual pictures of the carbon anode before and after electrolysis when no carbon anode antioxidant is used are shown respectively;
[0017] Figure 3 This is a physical picture of the carbon anode after the electrolytic aluminum experiment of Example 1;
[0018] Figure 4 This is a physical picture of the carbon anode after the aluminum electrolysis experiment of Example 2;
[0019] Figure 5 This is a physical picture of the carbon anode after the electrolytic aluminum experiment of Comparative Example 1. DETAILED DESCRIPTION
[0020] The invention provides a carbon anode antioxidant, which comprises, by weight percentage, 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite ore powder and 10% alumina powder.
[0021] In the present invention, the carbon anode antioxidant comprises, by mass percentage, 50% sodium silicate aqueous solution. In the present invention, the mass concentration of the sodium silicate aqueous solution is preferably 40-50%, more preferably 50%.
[0022] In the present invention, the carbon anode antioxidant comprises 10% asbestos felt by mass percentage. In the present invention, the asbestos felt is preferably in a flocculent state.
[0023] In the present invention, the carbon anode antioxidant comprises 30% fluorite powder by mass percentage, and the fluorite powder is preferably fluorite powder FC-97. In the present invention, the particle size of the fluorite powder is preferably ≤0.154 mm.
[0024] In the present invention, the carbon anode antioxidant includes 10% of alumina powder in terms of mass percentage, and the particle size of the alumina powder is preferably less than 150 μm.
[0025] In the present invention, the carbon anode antioxidant, measured by mass percentage, includes:
[0026] The present invention also provides a method for preparing a carbon anode antioxidant, comprising the following steps: mixing a sodium silicate aqueous solution, asbestos felt, fluorite ore powder and alumina powder to obtain the carbon anode antioxidant.
[0027] In the present invention, the mixing preferably includes: first mixing the sodium silicate aqueous solution and the asbestos felt, and second mixing the obtained first mixture with fluorite ore powder and alumina powder.
[0028] In the present invention, the first mixing method is preferably stirring, the stirring speed is preferably 170 to 350 rpm, more preferably 330 rpm, the stirring time is preferably 2 to 3 min, more preferably 3 min.
[0029] In the present invention, the second mixing method is preferably stirring, the stirring speed is preferably 170 to 350 rpm, more preferably 330 rpm, the stirring time is preferably 2 to 3 min, more preferably 3 min.
[0030] The present invention also provides the use of the carbon anode antioxidant in preventing carbon anode oxidation, and the application method is: before electrolysis, after applying the sodium silicate aqueous solution to the carbon anode, the carbon anode antioxidant is applied.
[0031] In the present invention, the sodium silicate aqueous solution is preferably coated to 1 mm. In the present invention, the thickness of the coated carbon anode antioxidant is preferably 0.4 to 0.6 cm, more preferably 0.5 cm.
[0032] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0033] Example 1
[0034] Carbon anode antioxidant:
[0035] Calculated by mass percentage, it is composed of 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite mineral powder (particle size is 0.154mm), and 10% alumina powder (particle size is <150μm).
[0036] The sodium silicate aqueous solution and asbestos felt of the above components were stirred and mixed at a rotation speed of 330 rpm for 3 minutes, and then stirred and mixed with fluorite ore powder and alumina powder at a rotation speed of 330 rpm for 3 minutes to obtain the carbon anode antioxidant.
[0037] After the surface of the carbon anode at the 4# feeding port of an electrolytic cell was cleaned with high-pressure wind, a layer of sodium silicate aqueous solution (1mm thick) was first applied to the surface of the carbon anode near the feeding port, and then a carbon anode antioxidant was applied with a thickness of about half a centimeter on the anode surface. After being placed in the electrolytic cell, an electrolytic aluminum experiment was carried out, and the conditions for electrolytic aluminum included: the electrolyte was cryolite solution, the current was 240KA, and the time was 32 days.
[0038] The carbon anode after the electrolytic aluminum experiment Figure 3 ,from Figure 3 It can be seen that: in addition to the carbon anode wrapped around the steel claw, the steel claw is not corroded by the electrolyte, the aluminum oxide block attached to its surface is relatively intact, the surface of the carbon anode retains the texture of the new anode part, with less consumption and good anti-oxidation effect.
[0039] Example 2
[0040] Carbon anode antioxidant:
[0041] Calculated by mass percentage, it is composed of 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite mineral powder (particle size is 0.154mm), and 10% alumina powder (particle size is <150μm).
[0042] The sodium silicate aqueous solution and asbestos felt of the above components were stirred and mixed at a rotation speed of 330 rpm for 3 minutes, and then stirred and mixed with fluorite ore powder and alumina powder at a rotation speed of 330 rpm for 3 minutes to obtain the carbon anode antioxidant.
[0043] After the surface of the carbon anode at the 4# feeding port of an electrolytic cell was cleaned with high-pressure wind, a layer of sodium silicate aqueous solution (1mm thick) was first applied to the surface of the carbon anode near the feeding port, and then a carbon anode antioxidant was applied with a thickness of about half a centimeter on the anode surface. After being placed in the electrolytic cell, an electrolytic aluminum experiment was carried out, and the conditions for electrolytic aluminum included: the electrolyte was cryolite solution, the current was 240KA, and the time was 32 days.
[0044] The carbon anode after the electrolytic aluminum experiment Figure 4 ,from Figure 4 It can be seen that: when testing at different feed ports of the electrolytic cell, the carbon material wrapping around the steel claws was intact after the carbon anode at the feed port was used, which was in line with the test expectations.
[0045] Comparative Example 1
[0046] Carbon anode antioxidant:
[0047] Calculated by mass percentage, it is composed of 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite mineral powder (particle size is 0.154mm), and 10% alumina powder (particle size is <150μm).
[0048] The sodium silicate aqueous solution and asbestos felt of the above components were stirred and mixed at a rotation speed of 330 rpm for 3 minutes, and then stirred and mixed with fluorite ore powder and alumina powder at a rotation speed of 330 rpm for 3 minutes to obtain the carbon anode antioxidant.
[0049] The surface of the carbon anode at the 1# feeding port of an electrolytic cell was cleaned with high-pressure air, and the carbon anode anti-oxidant was applied to the part of the carbon anode near the feeding port with a thickness of about half a centimeter on the anode surface. After being placed in the electrolytic cell, an electrolytic aluminum experiment was carried out. The conditions for electrolytic aluminum included: the electrolyte was cryolite solution, the current was 240KA, and the time was 32 days.
[0050] The carbon anode after the electrolytic aluminum experiment Figure 5 ,from Figure 5 It can be seen that if a layer of sodium silicate aqueous solution is not applied in advance, the carbon material around the steel claw will be damaged to a certain extent after the carbon anode is used after electrolysis.
[0051] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A carbon anode antioxidant, characterized in that: Calculated by mass percentage, it includes 50% sodium silicate aqueous solution, 10% asbestos felt, 30% fluorite mineral powder, and 10% alumina powder.
2. The carbon anode antioxidant according to claim 1, characterized in that: The mass concentration of the sodium silicate aqueous solution is 40-50%.
3. The carbon anode antioxidant according to claim 1, characterized in that: The particle size of the fluorite mineral powder is ≤0.154 mm.
4. The carbon anode antioxidant according to claim 3, characterized in that: The fluorite mineral powder is fluorite mineral powder FC-97.
5. The carbon anode antioxidant according to claim 1, characterized in that: The particle size of the aluminum oxide powder is less than 150 μm.
6. The method for preparing the carbon anode antioxidant according to any one of claims 1 to 5, characterized in that: The following steps are involved: The sodium silicate aqueous solution, asbestos felt, fluorite ore powder and alumina powder are mixed to obtain the carbon anode antioxidant.
7. The preparation method according to claim 6, characterized in that: The mixing comprises: first mixing the sodium silicate aqueous solution and the asbestos felt, and second mixing the obtained first mixture with fluorite ore powder and alumina powder.
8. The preparation method according to claim 7, characterized in that: The first mixing method is stirring, the stirring speed is 170-350 rpm, and the time is 2-3 min; the second mixing method is stirring, the stirring speed is 170-350 rpm, and the time is 2-3 min.
9. Use of the carbon anode antioxidant according to any one of claims 1 to 5 in preventing carbon anode oxidation, characterized in that: The application method is: before electrolysis, the sodium silicate aqueous solution is applied to the carbon anode, and then the carbon anode antioxidant is applied.
10. The use according to claim 9, characterized in that: The thickness of the coated carbon anode antioxidant is 0.4 to 0.6 cm.