Selective hydrogenation process and catalyst therefor
By using carbon-coated nickel nanoparticle composite material with an effective amount of thiourea as a catalyst, the problem of high selectivity hydrogenation nitrogen in catalytic hydrogenation reaction is solved, high activity and high selectivity are achieved, and the stability of the catalyst is strengthened and product purity, avoid contamination of toxic additives.
Patent Information
- Application Number
- CN202310630673.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
In catalytic hydrogenation reaction, how to achieve high selective hydrogenation of nitro and carbon-carbon unsaturated bonds on the benzene ring of the hydrogenated substrate, and the commonly used selective regulators in existing methods are toxic And it is difficult to completely remove, affecting the catalyst activity and product purity.
The carbon-coated nickel nanoparticle composite material with an effective amount of thiourea is used as a catalyst to improve the selectivity of the hydrogenation reaction by modifying the properties of the carbon layer, and reduce the mixing of toxic additives by washing the soluble or soluble solvent of thiourea. Optimize reaction conditions to improve catalytic activity and selectivity.
Achieve high selective hydrogenation of nitro in hydrogenated substrates, high catalyst activity and long life, product conversion rate is close to 100%, selectivity is about 95% to 100%, and thiourea is prevented from entering hydrogenated products to the maximum extent. .
Smart Images

Figure CN119059918A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a selective hydrogenation method and a catalyst thereof, and in particular to a method and a catalyst thereof for highly selective hydrogenation of a nitro group when a nitro group and a carbon-carbon unsaturated bond coexist on the benzene ring of a hydrogenation substrate. Background Art
[0002] Catalytic hydrogenation is a very important reaction in the field of chemistry. It refers to the reaction in which hydrogen molecules are added to unsaturated groups of organic compounds under the action of a catalyst. When there are two or more unsaturated groups in the hydrogenation substrate, how to selectively hydrogenate specific unsaturated groups has always been a research difficulty in the field of catalytic hydrogenation.
[0003] Commonly used hydrogenation catalysts in industry include platinum-carbon, palladium-carbon and Raney nickel. The metals of these catalysts are exposed to the reaction environment and are prone to agglomeration and poisoning. Carbon-coated metal nanocomposites are newly emerging catalytic hydrogenation materials. Their metals are tightly coated by graphene carbon shells with a thickness of generally less than 10nm. The adsorption of hydrogenation substrates in the hydrogenation reaction occurs on the carbon shell, making it have both the stability of nanocarbon materials and the high activity of metal nanomaterials.
[0004] Methods for adjusting the selectivity of hydrogenation reactions can be divided into two categories: one is to achieve this by modifying the properties of the metal center during the catalyst manufacturing process; the other is to achieve this by adding a selectivity regulator during the hydrogenation reaction. Regardless of the method, the purpose is achieved by directly changing the properties of the metal active center. Existing methods are all aimed at reactions directly catalyzed by metals, and there are few documents on adjusting the selectivity of hydrogenation reactions catalyzed by carbon-coated metal materials. CN114425341A and CN114426506A earlier disclosed the anti-sulfur poisoning performance of graphene-coated nickel nanoparticles, showing that the presence of sulfur-containing compounds did not significantly affect the hydrogenation activity of the catalyst.
[0005] Selective regulators are usually compounds containing nitrogen, sulfur, and phosphorus. These heteroatoms bind to the metal surface to selectively poison the highly active metal center, thereby inhibiting side reactions. The disadvantage is that these heteroatoms have a strong interaction with the metal, generally forming chemical adsorption bonds or directly reacting with the active center. Therefore, their type and dosage are very critical. Improper selection will cause the catalyst activity to drop seriously or even lose its catalytic ability. The existing technology usually can only add selective regulators during the reaction process. These toxic compounds are often present in the reaction product components, and it is difficult to completely remove them.
[0006] Aminostyrene is an important chemical raw material, which is synthesized industrially by selective hydrogenation of nitro compounds. Since it contains both nitro groups and easily reducible carbon-carbon unsaturated bonds, how to selectively reduce the nitro groups is the main difficulty in manufacturing such compounds. Liu et al. (Journal of Catalysis, 2017, 350: 218–225) used glucose as a carbon source to prepare a carbon-coated nickel catalyst for the selective hydrogenation of 3-nitrostyrene. When the conversion rate was > 95%, the selectivity was about 80%.
[0007] The preceding information is only for enhancement of understanding of the background of the invention and may contain information that is not known to a person of ordinary skill in the art. Summary of the invention
[0008] The first object of the present invention is to provide a method for highly selective hydrogenation of nitro groups when nitro groups and carbon-carbon unsaturated bonds coexist on the benzene ring of the hydrogenation substrate, wherein the catalyst used in the method is a carbon-coated nickel nanoparticle composite material. The second object of the present invention is to improve the catalytic hydrogenation activity on the basis of achieving the above-mentioned objects. The third object of the present invention is to reduce or avoid the disadvantage of toxic additives being mixed into the hydrogenation product on the basis of achieving the above-mentioned objects. The fourth object of the present invention is to provide a catalyst for achieving the above-mentioned objects.
[0009] To achieve the above object, the present invention provides the following technical solutions.
[0010] 1. A selective hydrogenation process comprising:
[0011] S1 provides a selective hydrogenation catalyst, wherein the catalyst is a composite material of carbon-coated nickel nanoparticles containing an effective amount of thiourea on the surface, the composite material comprises a core-shell structure having a shell layer and a core, the shell layer is a graphitized carbon layer, and the core is a nickel nanoparticle; based on the mass of the catalyst, the mass fraction of nickel is 20% to 85%;
[0012] S2: contacting the hydrogenation substrate and hydrogen with the catalyst to react under liquid phase catalytic hydrogenation conditions; the benzene ring of the hydrogenation substrate has both a nitro group and a carbon-carbon unsaturated bond.
[0013] 2. The method according to 1, wherein the mass fraction of thiourea in the catalyst of S1, calculated as sulfur, is 0.05% to 1%, preferably 0.1% to 0.6%, based on the mass of the catalyst.
[0014] 3. A method according to any of the above, wherein the mass fraction of nickel is 30% to 80%, preferably 40% to 70%, based on the mass of the catalyst.
[0015] 4. The method according to any of the above, wherein the pickling loss rate of the composite material of the carbon-coated nickel nanoparticles is ≤30%, preferably ≤10%.
[0016] 5. A method according to any of the above, wherein the composite material of carbon-coated nickel nanoparticles is a mesoporous and / or macroporous material.
[0017] 6. According to any of the above methods, the thickness of the graphitized carbon layer is 0.3 nm to 6 nm, preferably 1 nm to 3 nm.
[0018] 7. According to any of the above methods, wherein, when observed under a transmission electron microscope, the particle size of the nickel nanoparticles is 2 nm to 48 nm, preferably 4 nm to 28 nm.
[0019] 8. The method according to any of the preceding claims, wherein the hydrogenation substrate is nitrostyrene.
[0020] 9. A method according to any of the above, wherein the mass ratio of the catalyst to the hydrogenation substrate is 1:1 to 1:50, preferably 1:2 to 1:40.
[0021] 10. The method according to any of the above, wherein the concentration of the hydrogenation substrate in the solvent is 5 g / L to 600 g / L, preferably 8 g / L to 500 g / L.
[0022] 11. A method according to any of the above, wherein the liquid phase catalytic hydrogenation reaction is carried out in the presence of a solvent, the solvent is isopropanol and water, and the volume ratio of the two is 1:1 to 50:1.
[0023] 12. According to any of the aforementioned methods, wherein the catalytic hydrogenation reaction conditions include: reaction temperature of 50°C to 70°C; hydrogen pressure of 0.7MPa to 2.5MPa.
[0024] 13. A method according to any of the preceding claims, wherein the thiourea concentration in the liquid phase of S2 is less than 50 mg / L, preferably less than 35 mg / L.
[0025] 14. A method according to any of the preceding claims, wherein the catalyst in S1 is washed with a solvent that is readily soluble or dissolvable in thiourea.
[0026] 15. A selective hydrogenation catalyst, wherein the catalyst is a composite material of carbon-coated nickel nanoparticles containing an effective amount of thiourea on the surface, the composite material contains a core-shell structure with a shell layer and an inner core, the shell layer is a graphitized carbon layer, and the inner core is a nickel nanoparticle; based on the mass of the catalyst, the mass fraction of nickel is 20% to 85%.
[0027] 16. The catalyst according to 15, wherein the mass fraction of thiourea calculated as sulfur is 0.05% to 1%, preferably 0.1% to 0.6%, based on the mass of the catalyst.
[0028] 17. A catalyst according to any of the above, wherein the acid washing loss rate of the composite material of the carbon-coated nickel nanoparticles is ≤30%, preferably ≤10%.
[0029] 18. A catalyst according to any of the above, wherein the mass fraction of nickel is 30% to 80%, preferably 40% to 70%, based on the mass of the catalyst.
[0030] 19. The catalyst according to any of the preceding claims, wherein the catalyst has been washed with a solvent that is readily soluble or miscible with thiourea.
[0031] Compared with the prior art, the present invention has the following beneficial technical effects.
[0032] The present invention provides a highly selective hydrogenation method, which can highly selectively hydrogenate the nitro group when both the nitro group and the carbon-carbon unsaturated bond exist on the benzene ring of the hydrogenation substrate. The catalyst used in the method is simple to prepare and easy to control, the product does not spontaneously combust and can be stored in the air for a long time, and the catalyst has high activity and long life and is easier to separate from the reaction system; these characteristics make the present invention unique in industrial production and application.
[0033] The present invention improves the selectivity of the hydrogenation reaction by modifying the properties of the carbon layer coated on the metal, and the correlation between the hydrogenation activity and the selectivity is reduced, making it easier to manufacture and apply the catalyst. The present invention can achieve higher hydrogenation activity while ensuring selectivity through optimization.
[0034] Thiourea is a serious catalyst poison, and the product of the present invention will be used as an organic intermediate, and the presence of thiourea is very unfavorable for subsequent applications. The present invention can reduce the concentration of thiourea in the liquid phase to a minimum through further optimization, thereby preventing thiourea from being brought into the hydrogenation product to the greatest extent.
[0035] By using the hydrogenation method and catalyst of the present invention, when catalytically hydrogenating nitrostyrene, the conversion rate approaches and reaches 100%, and the selectivity is about 95% to 100%.
[0036] Other features and advantages of the present invention will be described in detail in the detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The X-ray diffraction spectrum of the catalyst prepared according to the method of Example 2 is shown in FIG. DETAILED DESCRIPTION
[0038] The present invention is described in detail below in conjunction with specific implementations, but it should be noted that the protection scope of the present invention is not limited by these specific implementations and principle explanations, but is determined by the claims.
[0039] In the present invention, except for the contents explicitly described, any matters or items not mentioned are directly applicable to the contents known in the art without any changes. Moreover, any embodiment described herein can be freely combined with one or more other embodiments described herein, and the technical solutions or technical ideas formed thereby are regarded as part of the original disclosure or record of the present invention, and should not be regarded as new contents not disclosed or anticipated herein, unless a person skilled in the art considers that the combination is obviously unreasonable.
[0040] All features disclosed in the present invention may be combined arbitrarily, and these combinations shall be understood as the contents disclosed or recorded in the present invention, unless a person skilled in the art considers that the combination is obviously unreasonable, and shall be deemed to be specifically disclosed and recorded in the present invention. The numerical points disclosed in this specification, unless otherwise specified, include not only the numerical points specifically disclosed in the embodiments, but also the endpoints of each numerical range in the specification, and the range of any combination of these numerical points shall be deemed to be the range disclosed or recorded in the present invention.
[0041] For technical and scientific terms in the present invention, those directly defined herein shall prevail; those not defined herein shall prevail according to the definitions in the documents introduced herein; the rest shall be understood according to the general meaning in the art.
[0042] The term "macroporous material" is defined as a porous material comprising a macroporous distribution peak.
[0043] The term "mesoporous material" is defined as a porous material comprising a mesopore distribution peak.
[0044] The term "macroporous and mesoporous materials" is defined as porous materials comprising macropore and mesopore distribution peaks.
[0045] The term "inert gas" is defined as a gas that does not appreciably affect the catalytic hydrogenation performance of the composite material.
[0046] The term "soluble" means that 1 g to 10 g are soluble in 100 of a solvent at the temperature of use.
[0047] The term "readily soluble" means that 10 g or more of the compound is soluble in 100 g of the solvent at the use temperature.
[0048] The term "optionally" means that it may be present or not, such as A and optionally B, which means "A and not B" or "both A and B".
[0049] The term "acid treatment" refers to the operation of washing the product generated after the high-temperature pyrolysis step with a non-oxidizing strong acid at nearly 100° C. for a long time when preparing the composite material of carbon-coated nickel nanoparticles.
[0050] The present invention hereby incorporates the contents of CN109304475A, CN109304476A, CN109304194A, CN202211348441.1 and CN202211347510.7 in their entirety.
[0051] A first aspect of the present invention provides a selective hydrogenation method comprising:
[0052] S1 provides a selective hydrogenation catalyst, wherein the catalyst is a composite material of carbon-coated nickel nanoparticles containing an effective amount of thiourea on the surface, the composite material comprises a core-shell structure having a shell layer and a core, the shell layer is a graphitized carbon layer, and the core is a nickel nanoparticle; based on the mass of the catalyst, the mass fraction of nickel is 20% to 85%;
[0053] S2: contacting the hydrogenation substrate and hydrogen with the catalyst to react under liquid phase catalytic hydrogenation conditions; the benzene ring of the hydrogenation substrate has both a nitro group and a carbon-carbon unsaturated bond.
[0054] The homogenization of the three-dimensional structure and electronic configuration of the active center is the key to improving the selectivity of the hydrogenation reaction. From this perspective, the selectivity of the single active center homogeneous catalyst is higher, but it brings about the problem of catalyst separation and reuse that is difficult to overcome. Therefore, from an industrial perspective, a heterogeneous catalyst still needs to be used. There are multiple metal active sites in the heterogeneous catalyst. The existing methods directly transform its metal components when improving the selectivity of the hydrogenation reaction, and make it "homogenized" to a certain extent by covering and poisoning some metal active sites, thereby achieving the purpose of improving the selectivity of the reaction, generally at the cost of permanently sacrificing some activity. The present invention has found that a carbon-coated nickel nanoparticle composite material containing thiourea on the surface is used as a hydrogenation catalyst. When a nitro group and a carbon-carbon unsaturated bond are simultaneously present on the benzene ring of the hydrogenation substrate, the nitro group on the benzene ring can be highly selectively hydrogenated, thereby achieving the purpose of the present invention.
[0055] According to the selective hydrogenation method of the first aspect of the present invention, the catalyst in S1 is a composite material of carbon-coated nickel nanoparticles containing an effective amount of thiourea on the surface. The "effective amount" means that when a nitro group and a carbon-carbon unsaturated bond coexist on the benzene ring of the catalytic hydrogenation substrate, the hydrogenation selectivity to the nitro group is enhanced, compared with a catalyst without thiourea and with the same other conditions.
[0056] According to the selective hydrogenation method of the first aspect of the present invention, in the catalyst of S1, the mass fraction of thiourea calculated as sulfur is 0.05% to 1%, preferably 0.1% to 0.8%, based on the mass of the catalyst.
[0057] According to the selective hydrogenation method of the first aspect of the present invention, there is no particular limitation on the manner of introducing thiourea onto the surface of the composite material of carbon-coated nickel nanoparticles, and those skilled in the art may use any suitable manner known in the art, such as impregnation.
[0058] The present invention provides a method for manufacturing the catalyst in S1, which comprises the steps of mixing and impregnating a composite material of carbon-coated nickel nanoparticles with a thiourea solution. The mixing temperature may be 60°C to 100°C; the mixing method may be ultrasonic or stirring; the mass ratio of the carbon-coated nickel nanoparticle composite material to thiourea is 2:1 to 100:1, preferably 4:1 to 80:1. The method further comprises optional post-processing steps, such as separation, washing and drying. The separation may be carried out by filtering or centrifugation; the washing is preferably carried out by water washing; and the drying is generally not more than 80°C.
[0059] According to the selective hydrogenation method of the first aspect of the present invention, the carbon-coated nickel nanoparticle composite material is basically composed of nickel, carbon, oxygen and optional nitrogen. It should be understood that the carbon-coated nickel nanoparticle composite material is mainly composed of zero-valent nickel and carbon; since the carbon source in the synthetic raw material contains oxygen, it is inevitable that a small amount of oxygen will be mixed in the surface carbon of the composite material; if the carbon source contains nitrogen, the surface carbon of the composite material will also contain a small amount of nitrogen; the composite material will also adsorb oxygen on the surface when stored in the air, a small amount or trace amount of nickel may exist in the form of oxidation, and impurities in the synthetic raw material may also cause a small amount or trace amount of other elements, but these factors have not been found to have a significant effect on the catalytic hydrogenation performance of the composite material in the present invention; the present invention believes that there is no need to specify these.
[0060] According to the selective hydrogenation method of the first aspect of the present invention, the carbon-coated nickel nanoparticle composite material is mainly composed of a core-shell structure having a shell layer and a core, the shell layer is a graphitized carbon layer, and the core is a nickel nanoparticle. It should be understood that a small amount of carbon matrix will be generated in the process of manufacturing the carbon-coated nickel nanoparticle composite material, which has no significant effect on the catalytic hydrogenation performance of the composite material in the present invention, and the present invention also believes that it is not necessary to specify the amount of the carbon matrix.
[0061] The structure, composition and preparation method of carbon-coated nickel nanoparticle composite materials are well known in the art. The present invention has no particular restrictions on the carbon-coated nickel nanoparticle composite materials used, and those materials known in the art can be used, preferably those materials and preparation methods disclosed in CN109304475A, CN109304476A, CN109304194A, CN202211348441.1 and CN202211347510.7.
[0062] The pores of the composite materials in the aforementioned documents are mainly mesopores, and mesoporous and macroporous materials can also be obtained by using a specific method, such as the method in CN 111185211A. In the present invention, the carbon-coated nickel nanoparticle composite material is preferably a mesoporous and / or macroporous material, and further preferably, the volume of the mesopores and / or macropores accounts for more than 80% of the total pore volume. The so-called mesopores and macropores are the macroscopic properties of the catalytic material tested, and have nothing to do with the tightness of the graphitized carbon layer coating the nickel nanoparticles.
[0063] According to the selective hydrogenation method of the first aspect of the present invention, the acid washing loss rate of the carbon-coated nickel nanocomposite material is ≤30%, preferably ≤10%. It is known in the art that the nickel that is not tightly coated can be removed by acid treatment to obtain a carbon-coated nickel nanoparticle composite material that is more tightly coated. Generally speaking, when other conditions are basically the same, the tightly coated composite material has more stable properties and higher selectivity for the catalytic reaction. Acid treatment can generally be performed with sulfuric acid or hydrochloric acid, the acid concentration can be 0.1 mol / L to 3 mol / L, and the treatment time can be 24h to 48h.
[0064] According to the selective hydrogenation method of the first aspect of the present invention, the thickness of the graphitized carbon layer is less than 10 nm, generally 0.3 nm to 6.0 nm, and preferably 1 nm to 3 nm.
[0065] According to the selective hydrogenation method of the first aspect of the present invention, under transmission electron microscopy, the particle size of the nickel nanoparticles is 2 nm to 48 nm, preferably 4 nm to 28 nm.
[0066] According to the selective hydrogenation method of the first aspect of the present invention, the crystal form of the nickel nanoparticles is a face-centered cubic lattice structure and / or a close-packed hexagonal lattice structure.
[0067] According to the selective hydrogenation method of the first aspect of the present invention, the hydrogenation substrate is nitrostyrene and its derivatives, wherein the nitro group can be located at the ortho position, para position or meta position of the olefin group, and the product is the corresponding aminostyrene and its derivatives.
[0068] Furthermore, the hydrogenation substrate can be selected from at least one of 2-nitrostyrene, 3-nitrostyrene, 4-nitrostyrene and derivatives thereof, and the corresponding product is at least one of 2-vinylaniline, 3-vinylaniline, 4-vinylaniline and derivatives thereof.
[0069] According to the selective hydrogenation method of the first aspect of the present invention, in S2, the mass ratio of the catalyst to the hydrogenation substrate can be 1:1 to 1:50, preferably 1:2 to 1:40, for example, 1:2, 1:5, 1:10, 1:15, 1:20, 1:25, 1:30, 1:35, 1:40, or any range therebetween.
[0070] According to the selective hydrogenation method of the first aspect of the present invention, the reaction in S2 is preferably carried out in the presence of a solvent. The present invention does not particularly limit the specific selection of the solvent, and those skilled in the art can select any suitable solvent known in the art. The solvent is preferably isopropanol and water, and the volume ratio of the two is preferably 1:1 to 50:1.
[0071] According to the selective hydrogenation method of the first aspect of the present invention, the present invention has a wide range of selection of the amount of the solvent, based on the environment required for the reaction. The concentration of the hydrogenation substrate in the solvent can be 5g / L to 600g / L, generally 8g / L to 300g / L.
[0072] According to the selective hydrogenation method of the first aspect of the present invention, the time of the catalytic hydrogenation reaction can be appropriately selected according to the temperature and the hydrogen pressure. Preferably, the time of the catalytic hydrogenation reaction is 20 min to 400 min, preferably 40 min to 360 min, for example, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 200 min, 250 min, 300 min, 320 min, 360 min, or any range therebetween.
[0073] According to the selective hydrogenation method of the first aspect of the present invention, the preferred conditions for the catalytic hydrogenation reaction are: reaction temperature of 50° C. to 70° C.; hydrogen pressure of 0.7 MPa to 2.5 MPa.
[0074] According to the selective hydrogenation method of the first aspect of the present invention, the thiourea concentration in the liquid phase of S2 is less than 50 mg / L, preferably less than 35 mg / L. The thiourea in the catalyst may enter the liquid phase of the reaction system, and this part of the thiourea is not good for the hydrogenation activity. Controlling the thiourea concentration in the liquid phase within the above range can make the hydrogenation activity higher.
[0075] According to the selective hydrogenation method of the first aspect of the present invention, the catalyst in S1 is washed with a soluble or soluble solvent of thiourea. Thiourea is a serious poison for metal catalysts and is very easy to chemically adsorb or react on the metal surface. For example, direct contact with nickel usually causes it to lose its activity. The effect of thiourea on the carbon surface is significantly different from the former, and the thiourea impregnated on the carbon surface can partially enter the reaction solvent. The present invention preferably washes away this part of thiourea with a soluble or soluble solvent to avoid thiourea from mixing into the hydrogenated product. The hydrogenated product of the present invention is generally used as an organic synthesis intermediate, and the presence of thiourea is extremely unfavorable for subsequent applications. The poisoning of the hydrogenation catalyst caused by thiourea is generally permanent. However, the present invention finds that when a large amount of thiourea is used to treat the catalyst to reduce its hydrogenation activity, washing it with a soluble or soluble solvent of thiourea can restore its high hydrogenation activity, which is a feature not seen in the prior art.
[0076] The second aspect of the present invention provides a selective hydrogenation catalyst, wherein the catalyst is a composite material of carbon-coated nickel nanoparticles containing an effective amount of thiourea on the surface, the composite material contains a core-shell structure with a shell layer and an inner core, the shell layer is a graphitized carbon layer, and the inner core is a nickel nanoparticle; based on the mass of the catalyst, the mass fraction of nickel is 20% to 85%.
[0077] According to the catalyst of the second aspect of the present invention, the mass fraction of thiourea calculated as sulfur is 0.05% to 1%, preferably 0.1% to 0.6%, based on the mass of the catalyst.
[0078] According to the catalyst of the second aspect of the present invention, the acid washing loss rate of the composite material of the carbon-coated nickel nanoparticles is ≤30%, preferably ≤10%.
[0079] According to the catalyst of the second aspect of the present invention, the mass fraction of nickel is 30% to 80%, preferably 40% to 70%, based on the mass of the catalyst.
[0080] According to the catalyst of the second aspect of the present invention, the catalyst is washed with a solvent which is readily soluble or dissolvable in thiourea.
[0081] The present invention will be described in detail below through examples.
[0082] The surface morphology of the material was characterized by transmission electron microscopy (TEM). The model of the TEM used was JEM-2100 (JEOL Ltd.), and the test conditions of the TEM were: the acceleration voltage was 200 kV.
[0083] The analysis of five elements, carbon (C), hydrogen (H), oxygen (O), nitrogen (N), and sulfur (S), was performed on the Elementar Micro Cube elemental analyzer. The specific operation method and conditions are as follows: the sample is burned at high temperature in the presence of oxygen, and the C, H, N, and S in the sample are converted into CO 2 , H 2 O、N 2 、SO 2 After removing the interference factors, the reaction gas is carried by the carrier gas into the chromatographic column for separation, and finally detected by the thermal conductivity cell. The analysis of oxygen element is to use high temperature decomposition, under the action of carbon catalyst, to convert the oxygen in the sample into CO, and then use the thermal conductivity detector to detect CO. The metal element content is the normalized result after deducting the carbon, hydrogen, oxygen, nitrogen and sulfur content of the material.
[0084] The XRD diffractometer used was an X'Pert Pro X-ray diffractometer purchased from PA Nalytical of the Netherlands, and the test conditions were: Cu target, Kα ray, tube voltage of 40 kV, tube current of 40 mA, and 2θ scanning range of 5° to 80°.
[0085] The specific surface area and pore distribution of the materials were determined by the Brunauer-Emmett-Taller method (BET, Quantachrome AS-6B analyzer).
[0086] The following preparation examples illustrate the preparation of the catalyst (sulfur-modified carbon-coated nickel nanocomposite material):
[0087] S1. Weigh 21.01 g of citric acid monohydrate and 14.55 g of basic nickel carbonate (the molar ratio of basic nickel carbonate calculated as nickel element to citric acid monohydrate calculated as carboxylate is 1:3) and add them into 150 mL of deionized water. Stir at 100 °C to obtain a homogeneous solution, continue heating and evaporating to dryness, and grind the obtained solid to obtain a precursor.
[0088] S2. The obtained precursor is placed in a porcelain boat, and then the porcelain boat is placed in the constant temperature zone of a tubular furnace, nitrogen is introduced, and the flow rate of nitrogen is 100 mL / min, and the temperature is increased to 600°C at a rate of 10°C / min. After keeping the constant temperature for 120 minutes, the heating is stopped, and the mixture is cooled to room temperature under a nitrogen atmosphere to obtain a carbon-coated nickel nanocomposite material.
[0089] S3, take 4g of the obtained carbon-coated nickel nanocomposite material and 0.8g of thiourea, add them into 20mL of deionized water, stir at 85°C for 90min, filter, and wash with deionized water several times. Transfer the obtained filter cake into an oven and dry it at 80°C to obtain the sulfur-modified carbon-coated nickel nanocomposite material.
[0090] The element analyzer determined that the S mass fraction in the sulfur-modified carbon-coated nickel nanocomposite material was 0.38%, and the normalized Ni mass fraction was 73.80%.
[0091] Preparation Example 2
[0092] S1. Weigh 4.38 g (15 mmol) of ethylenediaminetetraacetic acid and 1.85 g (20 mmol) of nickel hydroxide (the molar ratio of nickel hydroxide calculated as nickel element to diethylaminetetraacetic acid calculated as carboxylate is 1:3) and add them into 150 mL of deionized water. Stir at 75 °C to obtain a homogeneous solution, continue heating and evaporating to dryness, and grind the solid to obtain a precursor.
[0093] S2. Place the precursor obtained in step S1 in a porcelain boat, then place the porcelain boat in the constant temperature zone of a tube furnace, introduce nitrogen with a flow rate of 80 mL / min, and heat to 600°C at a rate of 3°C / min. Stop heating after keeping the temperature constant for 3 hours and cool to room temperature under a nitrogen atmosphere.
[0094] S3, add 60mL, 0.5mol / L H 2 SO 4 The solution was stirred and refluxed at 80°C for 6 h, then the solution was filtered, washed with deionized water until neutral, and the powder was placed in an oven at 100°C for 2 h to obtain a carbon-coated nickel nanocomposite material.
[0095] S4, taking 3g of the obtained carbon-coated nickel nanocomposite material and 0.15g of thiourea, adding them to 30mL of deionized water, stirring at 100°C for 90min, filtering, and washing with deionized water for multiple times. The obtained filter cake was transferred to an oven and dried at 100°C to obtain the sulfur-modified carbon-coated nickel nanocomposite material.
[0096] Figure 1 This is an X-ray diffraction spectrum of the sulfur-modified carbon-coated nickel nanocomposite prepared according to the method of Example 2. As can be seen from the figure, there are diffraction peaks corresponding to fcc-Ni and hcp-Ni in the spectrum, as well as diffraction peaks of carbon materials. Using the Scherrer formula, the average particle size of the nickel nanoparticles is 13.9nm.
[0097] The element analyzer determined that the S content in the sulfur-modified carbon-coated nickel nanocomposite material was 0.38%, and the normalized Ni content was 56.49%.
[0098] The following test example is used to illustrate the application of sulfur-modified carbon-coated nickel nanocomposite as a catalyst in catalytic hydrogenation reaction
[0099] Test Example 1
[0100] 50 mg of the sulfur-modified carbon-coated nickel nanocomposite prepared in Example 1, 298 mg of 4-nitrostyrene, 27 mL of isopropanol, and 3 mL of water were added to the reactor. H2 was introduced into the reactor for replacement 4 times, and H2 was introduced again. 2 The pressure in the reactor was set to 1.0 MPa, and the temperature was raised to the predetermined reaction temperature of 60°C. After the reaction was continued for 90 minutes, the heating was stopped, and the pressure was released after the temperature dropped to room temperature. The reactor was opened and the product was taken out for chromatographic analysis. The conversion rate of the reactants and the selectivity of the target product were calculated by the following formula:
[0101] Conversion rate (%) = mass of reactants reacted / amount of reactants added × 100%
[0102] Selectivity (%) = mass of target product / mass of reaction product × 100%
[0103] After analysis, it was found that the conversion rate of 4-nitrostyrene was 99.6%, and the selectivity of 4-vinylaniline was 95.8%.
[0104] Test Example 2
[0105] 50 mg of the sulfur-modified carbon-coated nickel nanocomposite prepared in Example 2, 298 mg of 4-nitrostyrene, 27 mL of isopropanol, and 3 mL of water were added to the reactor, and H 2 After replacing the reactor 4 times, H 2 The pressure in the reactor was set to 1.0 MPa, and the temperature was raised to the predetermined reaction temperature of 60°C. After the reaction was continued for 90 minutes, the heating was stopped, and the pressure was released after the temperature dropped to room temperature. The reactor was opened and the product was taken out for chromatographic analysis. The conversion rate of the reactants and the selectivity of the target product were calculated by the following formula:
[0106] Conversion rate (%) = mass of reactants reacted / amount of reactants added × 100%
[0107] Selectivity (%) = mass of target product / mass of reaction product × 100%
[0108] After analysis, it was found that the conversion rate of 4-nitrostyrene was 99.8%, and the selectivity of 4-vinylaniline was 94.5%.
[0109] It can be seen from Test Example 2 that, using the hydrogenation method and catalyst of the present invention, at 60° C. and 1 MPa hydrogen pressure, the reaction conversion rate is about 100% and the selectivity is about 95%. When the catalyst without thiourea and other conditions are the same catalyzes the hydrogenation reaction under the same conditions, the yield of 4-aminophenylethane reaches 8.60%.
[0110] It can be seen from test examples 1 and 2 that, using the hydrogenation method and catalyst of the present invention, at 60°C and 1 MPa hydrogen pressure, the reaction conversion rate is about 100% and the selectivity is about 95%. When adding thiourea to the reaction system to catalyze the hydrogenation reaction using a catalyst that does not contain thiourea and other conditions are the same, the reaction temperature needs to be increased by 20°C to 40°C to achieve a similar effect.
[0111] It can be seen from Test Examples 1 and 2 that acid washing or not has no significant effect on the hydrogenation method and catalyst of the present invention.
[0112] It can be seen from Test Examples 1 and 2 that by using the hydrogenation method and catalyst of the present invention, it is not necessary to add thiourea to the hydrogenation reaction system.
Claims
1. A selective hydrogenation process comprising: S1 provides a selective hydrogenation catalyst, wherein the catalyst is a composite material of carbon-coated nickel nanoparticles with an effective amount of thiourea on the surface, the composite material has a core-shell structure with a shell layer and a core, the shell layer is a graphitized carbon layer, and the core is a nickel nanoparticle; Based on the mass of the catalyst, the mass fraction of nickel is 20% to 85%; S2: contacting the hydrogenation substrate and hydrogen with the catalyst to react under liquid phase catalytic hydrogenation conditions; the benzene ring of the hydrogenation substrate has both a nitro group and a carbon-carbon unsaturated bond.
2. The method according to claim 1, characterized in that In the catalyst of S1, the mass fraction of thiourea calculated as sulfur is 0.05% to 1%, preferably 0.1% to 0.6%, based on the mass of the catalyst.
3. The method according to claim 1, characterized in that Based on the mass of the catalyst, the mass fraction of nickel is 40% to 70%.
4. The method according to claim 1, characterized in that: Observation under a transmission electron microscope shows that the particle size of the nickel nanoparticles is 4 nm to 28 nm.
5. The method according to claim 1, characterized in that The hydrogenation substrate is nitrostyrene.
6. The method according to claim 1, characterized in that The mass ratio of the catalyst to the hydrogenation substrate is 1:1 to 1:50; the concentration of the hydrogenation substrate in the solvent is 5 g / L to 600 g / L.
7. The method according to claim 1, characterized in that The liquid phase catalytic hydrogenation reaction is carried out in the presence of a solvent, wherein the solvent is isopropanol and water, and the volume ratio of the two is 1:1 to 50:
1.
8. The method according to claim 1, characterized in that The catalytic hydrogenation reaction conditions include: reaction temperature of 50° C. to 70° C.; hydrogen pressure of 0.7 MPa to 2.5 MPa.
9. The method according to claim 1, characterized in that: The thiourea concentration in the liquid phase of S2 is less than 50 mg / L, preferably less than 35 mg / L.
10. The method according to claim 1, characterized in that The catalyst in S1 is washed with a solvent which is readily soluble or miscible with thiourea.
11. A selective hydrogenation catalyst, wherein: The catalyst is a composite material of carbon-coated nickel nanoparticles with an effective amount of thiourea on the surface. The composite material contains a core-shell structure with a shell layer and a core. The shell layer is a graphitized carbon layer and the core is a nickel nanoparticle. Based on the mass of the catalyst, the mass fraction of nickel is 20% to 85%.
12. The catalyst according to claim 11, characterized in that Based on the mass of the catalyst, the mass fraction of thiourea calculated as sulfur is 0.05% to 1%, preferably 0.1% to 0.6%.
13. The catalyst according to claim 11, characterized in that Based on the mass of the catalyst, the mass fraction of nickel is 40% to 70%.
14. The catalyst according to claim 11, characterized in that The catalyst is washed with a solvent which is readily soluble or dissolvable in thiourea.
Citation Information
Patent Citations
Carbon-coated transition metal nano composite material and preparation method thereof as well as application
CN109304476A
Carbon-coated nickel nano composite material and preparation method thereof
CN111185211A
Method for synthesizing vinyl aniline compound with high selectivity
CN117964494A
Method for synthesizing 3-aminophenylacetylene
CN117964495A
Catalyst for selective hydrogenation reaction of aromatic nitrocompound and preparation method of catalyst
CN105032424A