Pyrene ring-containing alpha-diimine nickel catalyst as well as preparation method and application thereof

By designing a pyrene-containing nickel catalyst with α-diimine, the steric hindrance of the catalyst is adjusted by using the π-π stacking effect of the pyrene-ring ring, the problems of high branching degree and low molecular weight in olefin polymerization are solved, and the problem of existing catalysts is achieved. Higher polyolefin molecular weight and improved physical properties.

CN119059931AActive Publication Date: 2024-12-03UNIV OF SCI & TECH OF CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310630546.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

The existing catalysts have problems of high branching degree and low molecular weight during the olefin polymerization process, which affects the physical properties of polyolefin materials.

Method used

A pyrene-containing nickel catalyst is designed to adjust the steric steric resistance of the catalyst through the π-π stacking effect of the pyrene ring, reduce branching degree and increase molecular weight. The catalyst consists of an aromatic hydrocarbon body and a pyrene ring, formed by coordination with a divalent nickel salt, and is suitable for polymerization and copolymerization of ethylene and low-carbon olefins.

Benefits of technology

The stability and monomer activity of the catalyst are improved, the molecular weight of the polyolefin products is significantly improved, the branching degree is reduced, and the physical properties of the polyolefin materials are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004258250990000021
    Figure BDA0004258250990000021
  • Figure BDA0004258250990000022
    Figure BDA0004258250990000022
  • Figure BDA0004258250990000031
    Figure BDA0004258250990000031
Patent Text Reader

Abstract

The invention provides a pyrene ring-containing compound, a pyrene ring-containing alpha-diimine nickel catalyst as well as a preparation method and application of the pyrene ring-containing alpha-diimine nickel catalyst. The catalyst provided by the invention is a catalyst with a structure as shown in a formula (II), an imine compound is taken as an aromatic hydrocarbon main body, a pyrene ring is introduced to obtain a novel pyrene condensed ring aromatic hydrocarbon compound, and the novel pyrene ring-containing alpha-diimine nickel catalyst is obtained after the pyrene ring-containing alpha-diimine nickel catalyst is coordinated with a bivalent nickel salt. The prepared catalyst has good catalytic activity and thermal stability when being used for olefin polymerization reaction, and is suitable for a polymerization reaction system with polar monomers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalytic olefin polymerization and synthetic high molecular weight polyolefin materials, and in particular to a pyrene ring-containing α-diimine nickel catalyst and a preparation method and application thereof. Background Art

[0002] Polyolefin materials are rich in raw materials, low in price, easy to process and shape, and have excellent comprehensive properties. They are a type of polymer material with the largest output and the widest application. Among them, polyethylene material is a thermoplastic resin obtained by polymerization with ethylene as the main reactant. It has good chemical stability, excellent electrical insulation, and good resistance to low temperature and non-oxidizing acid corrosion. Since the early 1930s, after the earliest polyethylene product, low-density polyethylene, was obtained by free radical polymerization, polyolefin materials have gradually developed into synthetic polymer materials with the largest output, the most widespread use, and the lowest price. The main method for preparing polyethylene materials is the low-pressure method, and its core lies in the selection of catalysts. In the 1950s, Ziegler and Natta used coordination polymerization catalysts to achieve olefin polymerization under mild conditions, thereby promoting the vigorous development of the polyolefin industry.

[0003] As a type of coordination polymerization catalyst, transition metal catalysts have received great attention from academia and industry with the continuous development of the polyolefin industry. Among them, late transition metal catalysts represented by nickel and palladium have been widely studied in olefin polymerization and copolymerization of olefins with polar monomers due to their low oxygen affinity and high tolerance to polar groups. This type of catalyst has a unique "chain walking" feature and can prepare polyethylene with different branched structures and topological structures. Different combinations of compounds will have different effects on the performance of the compounds. Therefore, finding a new catalyst structure has far-reaching significance in the application of polyolefin industry. Summary of the invention

[0004] In view of this, in order to solve at least one of the technical problems described above and in other aspects of the related art, the present disclosure proposes a pyrene ring-containing α-diimine nickel catalyst and its preparation method and application, and designs and synthesizes a catalyst with an aromatic hydrocarbon as the main body and a structure with a π-π stacking effect, in which the pyrene ring adjusts the steric hindrance of the catalyst metal center, thereby optimizing its catalytic performance.

[0005] In one aspect of the present disclosure, a pyrene ring-containing compound is provided, the structure of which is shown in formula (I):

[0006]

[0007] Among them, R 1 ~R 5 is independently selected from one of hydrogen, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted phenyl, R1 ~R 5 Any two adjacent ones can form a loop with each other;

[0008] Z and Y are independently selected from one of hydrogen, C1-C6 alkyl, C1-C6 haloalkyl, substituted or unsubstituted phenyl. When Z and Y are selected from C1-C6 alkyl, C1-C6 haloalkyl, or substituted or unsubstituted phenyl, Z and Y can form a ring;

[0009] When the above substituted or unsubstituted group has a substituent, the substituent is selected from C1-C6 alkyl, phenyl or halogen.

[0010] According to the embodiment of the present disclosure, the ring structure of Z and Y includes substituted or unsubstituted following groups: one of acenaphthenyl, phenanthrenyl, C5-C8 cycloalkyl;

[0011] R 1 ~R 5 independently selected from methyl, ethyl, isopropyl or benzhydryl;

[0012] Z and Y are independently selected from hydrogen, methyl or form acenaphthene.

[0013] According to the embodiment of the present disclosure, its structural formula is shown in any one of the following formulas (I-1) to (I-3):

[0014]

[0015] In another aspect of the present disclosure, a pyrene ring-containing α-diimine nickel catalyst is provided, the structure of which is shown in formula (II),

[0016]

[0017] Among them, R 1 ~R 5 is independently selected from one of hydrogen, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted phenyl, R 1 ~R 5 Any two adjacent ones can form a loop with each other;

[0018] Z and Y are independently selected from one of hydrogen, C1-C6 alkyl, C1-C6 haloalkyl, substituted or unsubstituted phenyl. When Z and Y are selected from C1-C6 alkyl, C1-C6 haloalkyl, or substituted or unsubstituted phenyl, Z and Y can form a ring;

[0019] X is selected from halogen, C1-C6 alkyl, C2-C6 alkenyl, allyl, and benzyl;

[0020] When the above-mentioned substituted or unsubstituted group has a substituent, the substituent is selected from one of C1-C6 alkyl, phenyl and halogen.

[0021] According to the embodiments of the present disclosure, the ring-forming structure includes substituted or unsubstituted groups of the following: one of acenaphthenyl, phenanthrenyl, and C5-C8 cycloalkyl;

[0022] Preferably, Z and Y are independently selected from hydrogen or form acenaphthene;

[0023] Preferably, R 1 ~R 5 Independently selected from methyl, ethyl, isopropyl, diphenylmethyl;

[0024] Preferably, X is selected from halogen.

[0025] According to the embodiments of the present disclosure, the structural formula of the pyrene ring-containing α-diimine nickel catalyst is shown in any one of the following formulas (II-1) to (II-3):

[0026]

[0027] In another aspect of the present disclosure, a method for preparing the above catalyst is provided, comprising:

[0028] Dissolve the unilateral imine compound of formula (A), the aminopyrene compound of formula (B) and an organic acid catalyst in an aprotic solvent, and reflux for 24 to 72 hours to obtain a pyrene ring-containing compound of formula (I);

[0029] The pyrene ring-containing compound and the nickel salt are mixed in a molar ratio of 1:1 to obtain a pyrene ring-containing α-diimine nickel catalyst of formula (II);

[0030]

[0031] The aprotic solvent includes one of tetrahydrofuran, petroleum ether, toluene, benzene, dichloromethane, tetrachloromethane, ethyl ether, 1,4-dioxane and 1,2-dichloroethane;

[0032] Nickel salts including NiCl 2 、NiBr 2 , NiI 2 、(DME)NiBr 2 One of;

[0033] The organic acid catalyst includes one of trifluoroacetic acid, trichloroacetic acid, p-toluenesulfonic acid and methanesulfonic acid.

[0034] In another aspect of the present disclosure, a method for preparing polyethylene using the above catalyst is provided, comprising: adding a pyrene ring-containing α-diimine nickel catalyst liquid to ethylene in a protective gas atmosphere, reacting for 0.1 to 20 hours at 0 to 80° C. and 0.2 to 3 MPa to obtain polyethylene;

[0035] Preferably, the above method further comprises using a co-catalyst to assist the reaction, and the co-catalyst may be selected from: methylaluminoxane, diethylaluminum chloride, and the like.

[0036] According to an embodiment of the present disclosure, adding a pyrene ring-containing α-diimine nickel catalyst liquid into ethylene includes dissolving a pyrene ring-containing α-diimine nickel catalyst and a pyrene condensed ring aromatic hydrocarbon compound in a solvent at a ratio of 1:0.5 to 1:5 to obtain a catalyst mixed liquid, and adding the catalyst mixed liquid into ethylene;

[0037] Preferably, the pyrene-fused aromatic hydrocarbon compound includes one of pyrene, benzopyrene and coronene.

[0038] In another aspect of the present disclosure, a method for preparing a copolymer of a low-carbon olefin and methyl undecenoate using the above catalyst is proposed, comprising: in a protective gas atmosphere, mixing and dissolving a pyrene ring-containing α-diimine nickel catalyst with a low-carbon olefin and methyl undecenoate, and reacting for 0.1 to 20 hours under the conditions of 20 to 80° C. and 0.2 to 3 MPa to obtain a copolymer of a low-carbon olefin and methyl undecenoate; wherein the low-carbon olefin is C 2 -C 4 Olefins.

[0039] According to the embodiments of the present disclosure, an imine compound is used as the main aromatic hydrocarbon, and a pyrene ring is introduced to obtain a new pyrene-condensed aromatic hydrocarbon compound, which is coordinated with a divalent nickel salt to obtain a new pyrene-ring-containing α-diimine nickel catalyst. The steric hindrance of the nickel metal center in the catalyst is adjusted by the π-π stacking effect of the pyrene ring, thereby improving the catalyst stability, reducing the branching degree during olefin polymerization, and improving the monomer activity and the molecular weight of the polyolefin product. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 is a hydrogen nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 1 of the present disclosure;

[0041] Figure 2 is the carbon NMR spectrum of the pyrene ring-containing compound in Example 1 of the present disclosure;

[0042] Figure 3 is an electrospray ionization mass spectrum (ESI-MS) of the pyrene ring-containing compound in Example 1 of the present disclosure;

[0043] Figure 4 is the hydrogen nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 2 of the present disclosure;

[0044] Figure 5 is the electrospray mass spectrum of the pyrene ring-containing compound in Example 2 of the present disclosure;

[0045] Figure 6 is the hydrogen nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 3 of the present disclosure;

[0046] Figure 7 is the carbon NMR spectrum of the pyrene ring-containing compound in Example 3 of the present disclosure;

[0047] Figure 8 is the electrospray mass spectrum of the pyrene ring-containing compound in Example 3 of the present disclosure;

[0048] Fig. 9 is a matrix-assisted laser desorption ionization time-of-flight mass spectrometer (MALDI-TOF) of the pyrene ring-containing compound in Example 4 of the present disclosure;

[0049] Fig.10 is a matrix-assisted laser desorption ionization time-of-flight mass spectrum of the pyrene ring-containing compound in Example 5 of the present disclosure;

[0050] Fig.11 It is a matrix-assisted laser desorption ionization time-of-flight mass spectrum of the pyrene ring-containing compound in Example 6 of the present disclosure. DETAILED DESCRIPTION

[0051] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0052] The endpoints and any values ​​of the ranges disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this disclosure.

[0053] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0054] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification, and should not be interpreted in an idealized or overly rigid manner.

[0055] The "chain walking" feature of late transition metal catalysts refers to the catalytic activation through the dynamic displacement of the catalyst along the polymer backbone to the terminal position of the backbone. β-H elimination is a way of chain termination in polymerization reactions. Specifically, it refers to the metal center of the catalyst combining with the hydrogen on the β-carbon on the polymer chain to form a metal-hydrogen bond and separate the polymer backbone from the catalyst, thereby obtaining a polymer.

[0056] Therefore, using aromatic hydrocarbons as catalyst ligands is conducive to designing the structure of α-diimine nickel catalysts to obtain various branched chains and topological structures. At the same time, the introduction of pyrene ring structures with π-π stacking conjugation effect in late transition metal catalysts can effectively increase the steric hindrance of the catalyst. The increase in the steric hindrance of the metal catalyst will hinder the combination between β-H and the metal bond of the catalyst, allowing the polymer chain to continue to grow, thereby increasing the molecular weight of the polymer. The degree of branching is an important parameter affecting the physical properties of polyolefin materials. For the α-diimine catalyst system, the characteristics of its chain walking will cause the obtained polymer to produce branches. The mechanism of this process is mainly that the polymer chain that falls off after the elimination of β-H is reinserted into the metal center of the catalyst, and moves to the new polymer chain end with the catalyst to produce branches. The increase in catalyst steric hindrance will have an obstructive effect, so increasing the steric hindrance of the catalyst will reduce the degree of branching of the polyolefin material. There is no direct relationship between the catalyst activity and the steric hindrance effect, so a lot of searching, synthesis and testing are needed to explore the structure and performance of the catalyst.

[0057] In one aspect of the present disclosure, a pyrene ring-containing compound is provided, the structure of which is shown in formula (I):

[0058]

[0059] Among them, R 1 ~R 5 is independently selected from hydrogen, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted phenyl, R 1 ~R 5 Any two adjacent ones can form a loop with each other;

[0060] Z and Y are independently selected from one of hydrogen, C1-C6 alkyl, C1-C6 haloalkyl, substituted or unsubstituted phenyl. When Z and Y are selected from C1-C6 alkyl, C1-C6 haloalkyl, or substituted or unsubstituted phenyl, Z and Y can form a ring;

[0061] When the above substituted or unsubstituted group has a substituent, the substituent is selected from C1-C6 alkyl, phenyl or halogen.

[0062] According to the embodiment of the present disclosure, the ring structure of Z and Y includes substituted or unsubstituted following groups: one of acenaphthenyl, phenanthrenyl, C5-C8 cycloalkyl;

[0063] R 1 ~R 5 independently selected from methyl, ethyl, isopropyl or benzhydryl;

[0064] Z and Y are independently selected from hydrogen, methyl or form acenaphthene.

[0065] According to the embodiment of the present disclosure, its structural formula is shown in any one of the following formulas (I-1) to (I-3):

[0066]

[0067] In the embodiments of the present disclosure, pyrene ring-containing compounds with structural formulae (I-1) to (I-3) were synthesized and their structures were verified by nuclear magnetic resonance detection and mass spectrometry.

[0068] In another aspect of the present disclosure, a pyrene ring-containing α-diimine nickel catalyst is provided, the structure of which is shown in formula (II),

[0069]

[0070] Among them, R 1 ~R 5 is independently selected from hydrogen, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted phenyl, R 1 ~R 5 Any two adjacent ones can form a loop with each other;

[0071] Z and Y are independently selected from one of hydrogen, C1-C6 alkyl, C1-C6 haloalkyl, substituted or unsubstituted phenyl. When Z and Y are selected from C1-C6 alkyl, C1-C6 haloalkyl, or substituted or unsubstituted phenyl, Z and Y can form a ring;

[0072] X is selected from halogen, C1-C6 alkyl, C2-C6 alkenyl, allyl, and benzyl;

[0073] When the above-mentioned substituted or unsubstituted group has a substituent, the substituent is selected from one of C1-C6 alkyl, phenyl and halogen.

[0074] According to the embodiments of the present disclosure, an imine compound is used as the main aromatic hydrocarbon, and a pyrene ring is introduced to obtain a new pyrene-condensed aromatic hydrocarbon compound, which is coordinated with a divalent nickel salt to obtain a new pyrene-ring-containing α-diimine nickel catalyst. The steric hindrance of the nickel metal center in the catalyst is adjusted by the π-π stacking effect of the pyrene ring, thereby improving the catalyst stability, reducing the branching degree during olefin polymerization, and improving the monomer activity and the molecular weight of the polyolefin product.

[0075] According to the embodiments of the present disclosure, the ring-forming structure includes substituted or unsubstituted groups of the following: one of acenaphthenyl, phenanthrenyl, and C5-C8 cycloalkyl;

[0076] Preferably, Z and Y are independently selected from hydrogen or form acenaphthene;

[0077] Preferably, R 1 ~R 5 Independently selected from methyl, ethyl, isopropyl, diphenylmethyl;

[0078] Preferably, X is selected from halogen.

[0079] According to the embodiments of the present disclosure, the structural formula of the pyrene ring-containing α-diimine nickel catalyst is shown in any one of the following formulas (II-1) to (II-3):

[0080]

[0081] In the embodiments of the present disclosure, pyrene ring-containing α-diimine nickel catalysts with structural formulas such as (II-1) to (II-3) were synthesized and their structures were verified by nuclear magnetic resonance detection and mass spectrometry.

[0082] In another aspect of the present disclosure, a method for preparing the above catalyst is provided, comprising:

[0083] Dissolve the unilateral imine compound of formula (A), the aminopyrene compound of formula (B) and an organic acid catalyst in an aprotic solvent, and reflux for 24 to 72 hours to obtain a pyrene ring-containing compound of formula (I);

[0084] The pyrene ring-containing compound and the nickel salt are mixed in a molar ratio of 1:1 to obtain a pyrene ring-containing α-diimine nickel catalyst of formula (II);

[0085]

[0086]

[0087] The aprotic solvent includes one of tetrahydrofuran, petroleum ether, toluene, benzene, dichloromethane, tetrachloromethane, ethyl ether, 1,4-dioxane and 1,2-dichloroethane;

[0088] Nickel salts including NiCl2 、NiBr 2 , NiI 2 、(DME)NiBr 2 One of;

[0089] The organic acid catalyst includes one of trifluoroacetic acid, trichloroacetic acid, p-toluenesulfonic acid and methanesulfonic acid.

[0090] According to the embodiments of the present disclosure, the protic solvent will dissociate, affecting the pH of the reaction system.

[0091] In another aspect of the present disclosure, a method for preparing polyethylene using the above catalyst is provided, comprising: adding a pyrene ring-containing α-diimine nickel catalyst liquid to ethylene in a protective gas atmosphere, reacting for 0.1 to 20 hours at 0 to 80° C. and 0.2 to 3 MPa to obtain polyethylene;

[0092] Preferably, the above method further comprises using a co-catalyst to assist the reaction, and the co-catalyst may be selected from: methylaluminoxane, diethylaluminum chloride, and the like.

[0093] According to an embodiment of the present disclosure, adding a pyrene ring-containing α-diimine nickel catalyst liquid into ethylene includes dissolving a pyrene ring-containing α-diimine nickel catalyst and a pyrene condensed ring aromatic hydrocarbon compound in a solvent at a ratio of 1:0.5 to 1:5 to obtain a catalyst mixed liquid, and adding the catalyst mixed liquid into ethylene;

[0094] Preferably, the pyrene-fused aromatic hydrocarbon compound includes one of pyrene, benzopyrene and coronene.

[0095] According to the embodiments of the present disclosure, the addition of a pyrene-condensed aromatic compound and the use of the catalyst in the present disclosure can increase the steric hindrance of the catalyst to increase the molecular weight of the polyethylene product while reducing the degree of branching.

[0096] In another aspect of the present disclosure, a method for preparing a copolymer of a low-carbon olefin and methyl undecenoate using the above catalyst is proposed, comprising: in a protective gas atmosphere, mixing and dissolving a pyrene ring-containing α-diimine nickel catalyst with a low-carbon olefin and methyl undecenoate, and reacting for 0.1 to 20 hours under the conditions of 20 to 80° C. and 0.2 to 3 MPa to obtain a copolymer of a low-carbon olefin and methyl undecenoate; wherein the low-carbon olefin is C 2 -C 4 Olefins.

[0097] It should be noted that the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments of the present disclosure, other embodiments obtained by ordinary technicians in the field without creative work are all within the scope of protection of the present disclosure.

[0098] The following examples illustrate the specific content of the present disclosure, and the data provided include the synthesis of ligands, the synthesis of metal compounds, and the ethylene polymerization or copolymerization method, wherein the synthesis of the complex and the polymerization process are carried out under anhydrous and oxygen-free conditions, all sensitive substances are stored in a glove box, all solvents are strictly dried and dehydrated, and ethylene gas is purified by a dehydration and deoxygenation column. Unless otherwise specified, all compounds are commercially purchased and used in the present disclosure.

[0099] The nuclear magnetic resonance detection was performed by a Bruker 400 MHz nuclear magnetic resonance instrument, the molecular weight and molecular weight distribution were determined by high temperature gel permeation chromatography (GPC), and the mass spectrum was determined by a Thermo LTQ Orbitrap XL.

[0100] Example 1: Synthesis of Compound I-1

[0101] 5mmol of a unilateral imine compound as shown in formula (A-1) and 5mmol of a 1-aminopyrene compound as shown in formula (B-1) were mixed in a 200ml round-bottom flask, 100ml of toluene was added, and the mixture was placed in a 140°C oil bath to separate water and react for 24h. After the reaction was completed, the excess toluene was concentrated in vacuo, and the crude reaction product was separated by column chromatography to obtain a pyrene ring compound as shown in formula (Ⅰ-1). Among them, compound Ⅰ-1 was a yellow solid (0.89g, 2mmol), with a yield of 40%, and the separation column used a neutral alumina column (eluent EA / PE = 1 / 100).

[0102]

[0103] Compound I-1 was subjected to nuclear magnetic resonance detection to verify its specific structure, and electrospray ionization mass spectrometry was used to detect its structural multiply charged molecular ions to identify the macromolecular material.

[0104] Figure 1 It is the hydrogen nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 1 of the present disclosure.

[0105] like Figure 1 As shown, its hydrogen spectrum data is: 1 H NMR (400MHz, CD 2 Cl 2 )δ8.26-8.13(m,3H), 8.10-7.94(m,5H), 7.46(d,J=8.0Hz,1H), 7.19(d,J=7.4Hz,2H), 7.12(s,1H), 2.84-2.71(m,2H), 2.22(d,J=12.2Hz,6H), 1.21(dd,J=24.8,6.9Hz,12H).

[0106] Figure 2 It is the carbon nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 1 of the present disclosure.

[0107] like Figure 2 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, CD 2 Cl 2 )δ: 169.31,168.35,146.36,145.08,135.18,131.72,131.52,128.22,127.45,127.04,126.31,126.10,125.43,125.39,124. 99,124.76,123.94,123.11,122.71,120.87,116.46,54.11,53.84,53.57,53.30,53.03,28.49,23.12,22.68,16.47,16.11.

[0108] Figure 3 This is the electrospray mass spectrum of Example 1 of the present disclosure.

[0109] like Figure 3 As shown, its electrospray mass spectrometry data is: ESI-MS (m / z): 445.26316 [M+H] + .

[0110] Example 2: Synthesis of Compound I-2

[0111] 5mmol of a unilateral imine compound as shown in formula (A-2) and 5mmol of a 1-aminopyrene compound as shown in formula (B-2) were mixed in a 200ml round-bottom flask, 100ml of toluene was added, and the mixture was placed in a 140°C oil bath to separate water and react for 24h. After the reaction was completed, the excess toluene was concentrated in vacuo, and the crude reaction product was separated by column chromatography to obtain a pyrene ring compound as shown in formula (Ⅰ-2). Among them, compound Ⅰ-2 was an orange-yellow solid (0.98g, 1.8mmol), with a yield of about 36%, and the separation column used a neutral alumina column (eluent EA / PE = 1 / 100).

[0112]

[0113] Compound I-2 was subjected to nuclear magnetic resonance detection to verify its specific structure, and electrospray ionization mass spectrometry was used to detect its structural multiply charged molecular ions to identify the macromolecular material.

[0114] Figure 4 It is the hydrogen nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 2 of the present disclosure.

[0115] like Figure 4 As shown, its hydrogen spectrum data is: 1 H NMR (400MHz, CD 2 Cl 2 )δ8.32(d,J=8.1Hz,1H),8.14(d,J=6.7Hz,2H),8.09(dd,J=8.2,4.8Hz,2H),8.0 2(d,J=9.0Hz,2H),7.97-7.92(m,1H),7.84(dd,J=14.8,6.7Hz,2H),7.41-7.27(m ,4H),7.08(t,J=7.8Hz,1H),6.90(d,J=4.3Hz,1H),6.71(d,J=7.4Hz,1H),6.48( t,J=7.0Hz,1H),3.23-3.05(m,2H),1.31(d,J=6.8Hz,6H),1.06(d,J=6.9Hz,6H).

[0116] Figure 5 This is the electrospray mass spectrum of Example 1 of the present disclosure.

[0117] like Figure 5 As shown, its electrospray mass spectrometry data is: ESI-MS (m / z): 541.26320 [M+H] + .

[0118] Example 3: Synthesis of Compound I-3

[0119] 5mmol of the unilateral imine compound shown in formula (A-3), 5.5mmol of anhydrous zinc chloride and 15mL of glacial acetic acid were added to a 100mL round-bottom flask and stirred at 120°C for 30 minutes. Then 5mmol of the 1-aminopyrene compound shown in formula (B-1) was added, the temperature was raised to 140°C, and the reaction was refluxed for 3h. After the reaction was completed, the excess toluene was concentrated in vacuo, and the crude reaction product was separated by column chromatography to obtain a pyrene ring compound of formula (Ⅰ-3). Among them, compound Ⅰ-3 was a reddish brown solid (1.6g, 2.0mmol), with a yield of 40%, and the separation column used a neutral alumina column (eluent EA / PE = 1 / 100).

[0120]

[0121] Compound I-1 was subjected to nuclear magnetic resonance detection to verify its specific structure, and electrospray ionization mass spectrometry was used to detect its structural multiply charged molecular ions to identify the macromolecular material.

[0122] Figure 6 This is the hydrogen nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 3 of the present disclosure.

[0123] like Figure 6As shown, its hydrogen spectrum data is: 1 H NMR (400MHz, CD 2 Cl 2 )δ8.35(d,J=8.2Hz,1H),8.26-8.16(m,4H),8.10(t,J=7.9Hz,2H),8.05-8.00(m,1H),7.83-7.69(m,3H),7.44-7.36(m,4H),7.31(d,J=7.3Hz ,6H),7.13(d,J=7.5Hz,4H),7.02-6.97(m,1H),6.97-6.82(m,7H),6.6 6(dd,J=13.3,6.9Hz,3H),6.39-6.31(m,1H),5.76(s,2H),2.34(s,3H).

[0124] Figure 7 This is the carbon nuclear magnetic resonance spectrum of the pyrene ring-containing compound in Example 3 of the present disclosure.

[0125] like Figure 7 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, CD 2 Cl 2 )δ162.70,161.85,146.63,146.38,143.35,142.48,140.91,132.58,131.99,131.74,13167 ,130.45,130.05,129.90,12965,129.39,129.13,128.92,128.77,128.70,128.46,128.40, 128.26,127.89,127.79,127.52,127.29,127.07,126.91,126.30,126.13,125.77,125.69,124.92,124.72,123.78,122.95,115.67,54.03,53.76,53.49,53.22,52.95,52.50,21.32.

[0126] Figure 8 This is the electrospray mass spectrum of Example 3 of the present disclosure.

[0127] like Figure 8 As shown, its electrospray mass spectrometry data is: ESI-MS (m / z): 803.34088 [M+H] + .

[0128] Example 4: Synthesis of Catalyst II-1

[0129]

[0130] In a glove box, 1 mmol of compound Ⅰ-1 and 1 mmol of ethylene glycol dimethyl ether nickel bromide were placed in a 100 mL Shrek bottle, and then 30 mL of anhydrous dichloromethane was added and reacted at room temperature for 12 hours. After the reaction was completed, the solvent was removed by vacuum concentration, and anhydrous n-hexane was added for recrystallization. After filtration, the solid was washed three times with n-hexane to obtain a pyrene ring-containing catalyst as shown in formula (Ⅱ-1). Among them, catalyst Ⅱ-1 is an orange-red solid (0.56 g, 0.85 mmol) with a yield of about 85%.

[0131] Fig. 9 It is the matrix-assisted laser desorption ionization time-of-flight mass spectrometer in Example 4 of the present disclosure.

[0132] like Fig. 9 As shown, MALDI-TOF (m / z) data is: 583.500 [M-Br] + Elemental analysis: C 32 H 32 Br 2 N 2 Ni; C, 57.86; H, 4.95; N, 4.20.

[0133] Example 5: Synthesis of Catalyst II-2

[0134]

[0135] In a glove box, 1 mmol of compound Ⅰ-2 and 1 mmol of ethylene glycol dimethyl ether nickel bromide were placed in a 100 mL Shrek bottle, and then 30 mL of anhydrous dichloromethane was added and reacted at room temperature for 12 hours. After the reaction was completed, the solvent was removed by vacuum concentration, and anhydrous n-hexane was added for recrystallization. After filtration, the solid was washed three times with n-hexane to obtain a pyrene ring-containing catalyst as shown in formula (Ⅱ-2). Among them, catalyst Ⅱ-2 was a dark red solid (0.65 g, 0.85 mmol) with a yield of about 85%.

[0136] Fig.10 This is the matrix-assisted laser desorption ionization time-of-flight mass spectrometer in Example 5 of the present disclosure.

[0137] like Fig.10 As shown, the MALDI-TOF (m / z) data is: 679.272 [M-Br] + ; Elemental analysis: C 40 H 32 Br 2 N 2 Ni; C, 63.22; H, 4.15; N, 3.75.

[0138] Example 6: Synthesis of Catalyst II-3

[0139]

[0140] In a glove box, 1 mmol of compound Ⅰ-3 and 1 mmol of ethylene glycol dimethyl ether nickel bromide were placed in a 100 mL Shrek bottle, and then 30 mL of anhydrous dichloromethane was added and reacted at room temperature for 12 hours. After the reaction was completed, the solvent was removed by vacuum concentration, and anhydrous n-hexane was added for recrystallization. After filtration, the solid was washed three times with n-hexane to obtain a pyrene ring-containing catalyst as shown in formula (Ⅱ-3). Among them, catalyst Ⅱ-3 is a dark red solid (0.82 g, 0.80 mmol) with a yield of about 80%.

[0141] Fig.11 This is the matrix-assisted laser desorption ionization time-of-flight mass spectrometer in Example 6 of the present disclosure.

[0142] like Fig.11 As shown, MALDI-TOF (m / z) data is: 941.163 [M-Br] + , elemental analysis: C 61 H 42 Br 2 N 2 Ni; C, 71.81; H, 4.05; N, 2.76.

[0143] Application Example 1

[0144] The catalysts prepared in Examples 4-6 were used to carry out ethylene polymerization, and the specific polymerization method was as follows:

[0145] In a glove box with a nitrogen atmosphere, 28 mL of n-heptane and 0.25 mmol of diethylaluminum chloride were added to a 350 mL autoclave equipped with a magnetic stirring device, an oil bath heating device and a thermometer. The container was connected to a high-pressure pipeline and the pipeline was evacuated. The container was heated to 20°C with a water bath and kept warm for 10 minutes.

[0146] 2 mL of a dichloromethane solution containing 0.5 μmol of the catalyst prepared in Example 4-6 was injected into the container using a syringe, the valve was closed, and the ethylene pressure was adjusted to 8 atmospheres, and the reaction was carried out for 10 minutes.

[0147] The reaction was stopped, the reactor was opened, ethanol was added thereto to precipitate solids, and the solids were filtered and dried under reduced pressure to obtain white polyethylene solids.

[0148] In this application example, under the same conditions, the catalyst prepared in the example was not added, and 2 equivalents of pyrene were added as a control group, and it was found that no polyethylene was produced. That is, pyrene alone has no catalytic activity.

[0149] The results of ethylene polymerization catalyzed by the catalysts prepared in Examples 4-6 are shown in Table 1:

[0150] Table 1. Nickel complexes in Examples 4-6 a Ethylene homopolymerization

[0151]

[0152]

[0153] in, a Polymerization conditions: catalyst dosage: 0.5 μmol, diethylaluminum chloride dosage: 500 equivalents, n-heptane dosage: 28 ml, dichloromethane dosage: 2 ml, ethylene partial pressure: 8 bar, reaction time: 10 min;

[0154] b Active units: 10 6 g·(mol Ni) -1 ·h -1 ;

[0155] c The molecular weight and molecular weight polydispersity coefficient were determined by gel permeation chromatography (GPC) using polystyrene as a standard sample in 1,2,4-trichlorobenzene as a solvent at 160°C;

[0156] d The degree of branching was determined by H NMR spectroscopy;

[0157] e Melting points were determined by differential scanning calorimetry (DSC);

[0158] f Amount of added pyrene: 0.5 equivalent:

[0159] gAmount of added pyrene: 2.0 equivalents.

[0160] In the experiments No. 1-3 listed in Table 1, no pyrene-condensed aromatic hydrocarbon compound was added to the catalyst; in the experiments No. 4-9, pyrene-condensed aromatic hydrocarbon was added to the catalyst.

[0161] It can be seen from the data in Table 1 that under the regulation of added pyrene, the steric hindrance of the catalyst is increased, so that the molecular weight of the polyethylene product is significantly improved and the degree of branching is significantly reduced.

[0162] Application Example 2

[0163] The catalysts prepared in Examples 4-6 were used to carry out copolymerization of ethylene and polar monomers. The specific experimental steps and results are shown in Table 2:

[0164] Table 2 Nickel complexes in Examples 4-6a Copolymerization of ethylene with polar monomers under

[0165]

[0166]

[0167] in: a Polymerization conditions: catalyst dosage: 10 μmol, diethylaluminum chloride dosage: 1000 equivalents, ethylene polymerization conditions: 0.8 MPa, 10-undecenoic acid methyl ester 0.2 mol / L, 20°C, toluene 28 mL, 60 minutes;

[0168] b Active units: 10 5 g / (mol cat.×h);

[0169] c Melting point of copolymer;

[0170] d The mole fraction of polar monomer units in the copolymer;

[0171] e Number average molecular weight unit: kg / mol.

[0172] It can be seen from Table 2 that the catalyst prepared in the present disclosure can catalyze the copolymerization of ethylene and polar monomers to prepare polar polyolefins under certain conditions. The highest catalyst activity is 3.3×10 5 gmol -1 h -1 The melting point of ethylene copolymer is 105.9~111.1℃, and the maximum number average molecular weight is 14.5×10 3 g / mol.

[0173] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A pyrene ring-containing compound, the structure of which is shown in formula (I), in, R1-R5 are independently selected from one of hydrogen, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted phenyl, and any two adjacent R1-R5 can form a ring with each other; Z and Y are independently selected from one of hydrogen, C1-C6 alkyl, C1-C6 haloalkyl, substituted or unsubstituted phenyl. When Z and Y are selected from C1-C6 alkyl, C1-C6 haloalkyl, or substituted or unsubstituted phenyl, Z and Y can form a ring; When the above substituted or unsubstituted group has a substituent, the substituent is selected from C1-C6 alkyl, phenyl or halogen.

2. The compound according to claim 1, wherein The ring structure of Z and Y includes substituted or unsubstituted groups: one of acenaphthenyl, phenanthrenyl, and C5-C8 cycloalkyl; R1 to R5 are independently selected from methyl, ethyl, isopropyl or diphenylmethyl; Z and Y are independently selected from hydrogen, methyl or form acenaphthene.

3. The compound according to claim 1, wherein Its structural formula is shown in any one of the following formulas (I-1) to (I-3):

4. A pyrene ring-containing α-diimine nickel catalyst, the structure of which is shown in formula (II), in, R1-R5 are independently selected from one of hydrogen, halogen, substituted or unsubstituted C1-C6 alkyl, substituted or unsubstituted phenyl, and any two adjacent R1-R5 can form a ring with each other; Z and Y are independently selected from one of hydrogen, C1-C6 alkyl, C1-C6 haloalkyl, substituted or unsubstituted phenyl. When Z and Y are selected from C1-C6 alkyl, C1-C6 haloalkyl, or substituted or unsubstituted phenyl, Z and Y can form a ring; X is selected from halogen, C1-C6 alkyl, C2-C6 alkenyl, allyl, and benzyl; When the above substituted or unsubstituted group has a substituent, the substituent is selected from one of C1-C6 alkyl, phenyl and halogen.

5. The catalyst according to claim 4, wherein The ring-forming structure includes substituted or unsubstituted groups: one of acenaphthenyl, phenanthrenyl, and C5-C8 cycloalkyl; Preferably, Z and Y are independently selected from hydrogen or form acenaphthene; Preferably, R1 to R5 are independently selected from one of methyl, ethyl, isopropyl, and diphenylmethyl; Preferably, X is selected from halogen.

6. The catalyst according to claim 4, wherein Its structural formula is shown in any one of the following formulas (II-1) to (II-3):

7. A method for preparing the catalyst according to any one of claims 4 to 6, comprising: Dissolve the unilateral imine compound of formula (A), the aminopyrene compound of formula (B) and an organic acid catalyst in an aprotic solvent, and reflux for 24 to 72 hours to obtain a pyrene ring-containing compound of formula (I); The pyrene ring-containing compound and the nickel salt are mixed in a molar ratio of 1:1 to obtain a pyrene ring-containing α-diimine nickel catalyst of formula (II); Wherein, the aprotic solvent comprises one of tetrahydrofuran, petroleum ether, toluene, benzene, dichloromethane, tetrachloromethane, ethyl ether, 1,4-dioxane and 1,2-dichloroethane; The nickel salt includes one of NiCl2, NiBr2, NiI2, and (DME)NiBr2; The organic acid catalyst comprises one of trifluoroacetic acid, trichloroacetic acid, p-toluenesulfonic acid and methanesulfonic acid.

8. A method for preparing polyethylene using the catalyst according to any one of claims 4 to 6, comprising: In a protective gas atmosphere, the pyrene ring-containing α-diimine nickel catalyst liquid is added to ethylene, and the reaction is carried out at 0-80° C. and 0.2-3 MPa for 0.1-20 hours to obtain polyethylene; Preferably, the method further comprises using diethylaluminum chloride as a co-catalyst.

9. The method according to claim 8, wherein: Adding the pyrene ring-containing α-diimine nickel catalyst liquid into ethylene comprises: dissolving the pyrene ring-containing α-diimine nickel catalyst and a pyrene condensed ring aromatic hydrocarbon compound in a solvent at a ratio of 1:0.5 to 1:5 to obtain a catalyst mixed liquid, and adding the catalyst mixed liquid into ethylene; Preferably, the pyrene-fused aromatic hydrocarbon compound includes one of pyrene, benzopyrene and coronene.

10. A method for preparing a copolymer of light olefins and methyl undecenoate using the catalyst according to any one of claims 4 to 6, comprising: In the protective gas atmosphere, the pyrene ring-containing α-diimine nickel catalyst is mixed and dissolved with low-carbon olefins and methyl undecenoate, and reacted for 0.1 to 20 hours under the conditions of 20 to 80° C. and 0.2 to 3 MPa to obtain a copolymer of low-carbon olefins and methyl undecenoate; Among them, low carbon olefins are C2-C4 olefins.

Citation Information

Patent Citations

  • Naphthalene nucleus containing alpha-diketiminato nickel (II) composition as well as preparation method and application thereof

    CN102050840A

  • 4,4'-difluorobenzhydryl containing asymmetric alpha-diimine nickel complex, and intermediate, preparation method and application thereof

    CN106632506A

  • Asymmetric nickel diimide catalysts and ligands thereof, and preparation methods and applications thereof

    CN108912009A

  • Large steric hindrance diimine nickel catalyst and ligand thereof, and preparation method and application thereof