Method for preparing tetrahydrofurfuryl alcohol through furfural hydrogenation
A catalyst supported by basic carriers like La2O3, La(OH)3, or La2O2CO3, with active metals and auxiliary agents, effectively inhibits furfural polymerization and simplifies the separation of tetrahydrofurfuryl alcohol, achieving high yield and reducing environmental impact.
Patent Information
- Application Number
- CN202411151780.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-12-03
AI Technical Summary
Furfural easily polymerizes under acidic and heated conditions, leading to catalyst deactivation, and the separation of tetrahydrofurfuryl alcohol from water is energy-intensive, while existing methods generate significant inorganic alkali wastewater.
A method for preparing tetrahydrofurfuryl alcohol using a catalyst supported by a basic carrier, comprising La2O3, La(OH)3, or La2O2CO3, with active metals like Ni, Cu, or Pd, and auxiliary agents like Ca, Mg, Sr, Ba, Cd, Fe, Ru, Zn, or Al, to inhibit polymerization and facilitate easy separation.
The method achieves high yield of tetrahydrofurfuryl alcohol with a stable catalyst and reduces environmental impact by minimizing wastewater generation and energy consumption in separation.
Smart Images

Figure BDA0005003847720000051 
Figure BDA0005003847720000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of tetrahydrofurfuryl alcohol preparation, and particularly relates to a method for preparing tetrahydrofurfuryl alcohol by catalyzing furfural hydrogenation with a metal catalyst supported by an alkaline carrier. Background Art
[0002] Furfural, whose scientific name is α-furfurylaldehyde, is a derivative in which the hydrogen atom at the 2nd position of furan is replaced by an aldehyde group. It has active chemical properties and can be synthesized through oxidation, hydrogenation, condensation and other reactions. It is widely used in synthetic plastics, medicine, pesticides and other fields. Tetrahydrofurfuryl alcohol is an excellent solvent and an important fine chemical raw material. For example, it can be used as a solvent for coatings, resins and oils; it can also be used as a raw material for the preparation of pyridine, tetrahydrofuran, lysine, 1,5-pentanediol, etc.; it can also be used to prepare plasticizers, antifreeze, herbicides, pesticides, etc. Furfural can be obtained by hydrogenation reaction.
[0003] Furfural is very easy to undergo polymerization reaction under acidic and heated conditions, and the polymer is easy to accumulate on the catalyst, resulting in the deactivation of the catalyst. Chinese invention patent CN104672185A discloses that an inorganic base such as NaOH, Ca(OH)2, etc. is added to the furfural aqueous hydrogenation reaction to obtain a higher yield of tetrahydrofurfuryl alcohol, but a large amount of inorganic alkali wastewater is generated. At the same time, tetrahydrofurfuryl alcohol has a high solubility in water, and separating the tetrahydrofurfuryl alcohol product from water consumes a lot of energy. Summary of the invention
[0004] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing tetrahydrofurfuryl alcohol by hydrogenating furfural using a basic carrier-supported metal catalyst. The catalyst is simple to synthesize, the raw material price is low, the yield of tetrahydrofurfuryl alcohol is high, and it is easy to realize industrial production, and has commercial promotion and application value.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] The invention provides a method for preparing tetrahydrofurfuryl alcohol by hydrogenating furfural. Under the catalytic action of a catalyst, furfural and hydrogen are contacted and reacted to obtain tetrahydrofurfuryl alcohol. The catalyst comprises a carrier, an active metal and an auxiliary agent, wherein the carrier is at least one of La2O3, La(OH)3 and La2O2CO3, the active metal is at least one of Ni, Cu and Pd, and the auxiliary agent is at least one of Ca, Mg, Sr, Ba, Cd, Fe, Ru, Zn and Al.
[0007] Based on the above technical solution, further, the active metal accounts for 0.2-20% of the total mass of the catalyst, and the auxiliary agent accounts for 0-10% of the total mass of the catalyst.
[0008] Based on the above technical solution, further, the active metal accounts for 5-15% of the total mass of the catalyst, and the auxiliary agent accounts for 0.5-5% of the total mass of the catalyst.
[0009] Based on the above technical solution, further, the preparation of the catalyst includes the following steps: loading the active metal and the auxiliary agent onto the carrier by an impregnation method, and calcining and reducing the obtained solid in sequence after aging.
[0010] Based on the above technical solution, further, the aging temperature is 30-120°C, the aging time is 10-36h, the roasting temperature is 300-600°C, the roasting time is 1-5h, the reduction temperature is 300-500°C, and the reduction time is 1-5h.
[0011] Based on the above technical scheme, further, the impregnation method is one of co-impregnation and two-step impregnation. The specific process of the co-impregnation is to impregnate the metal salt precursor solution containing the active metal and the metal salt precursor solution of the auxiliary agent into the carrier; the specific process of the two-step impregnation is to first impregnate the metal salt precursor solution containing the active metal or the metal salt precursor solution containing the auxiliary agent into the carrier, and after aging and calcination, impregnate another solution, and then perform calcination and reduction treatment.
[0012] Based on the above technical solution, further, the metal salt precursor of the active metal is one or a combination of two or more of the nitrate, sulfate, chloride and acetate of the active metal, and the metal salt precursor of the auxiliary agent is one or a combination of two or more of the nitrate, sulfate, chloride and acetate of the auxiliary agent.
[0013] Based on the above technical solution, further, the contact reaction is specifically carried out by passing hydrogen and a solution containing furfural into a fixed bed reactor, the reaction temperature is 50-200°C, preferably 80-140°C, the pressure of hydrogen is 0.5-6MPa, preferably 1-3MPa, and the liquid space velocity of the solution containing furfural is 0.1-2h -1 , preferably 0.3-0.8h -1 , the molar ratio of hydrogen to furfural is (20-500):1.
[0014] Based on the above technical solution, further, the solvent of the solution containing furfural is one or a mixed solvent of two or more selected from water, ethanol, methanol, isopropanol, 1,4-dioxane, tetrahydrofuran and acetonitrile.
[0015] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0016] (1) The present invention uses rare earth La oxide as a carrier, which is cheap and readily available;
[0017] (2) La oxide is alkaline and can effectively inhibit furfural polymerization, reduce the generation of carbon deposits during the reaction, and is beneficial to the stability of the catalyst;
[0018] (3) Adding additives to the catalyst is beneficial to improving the dispersion of the metal and the activity of the catalyst;
[0019] (4) Compared with inorganic alkaline solutions, alkaline oxides are less polluting and are beneficial to the separation of tetrahydrofurfuryl alcohol products after the reaction. DETAILED DESCRIPTION
[0020] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0021] Analysis and detection methods: Agilent 7890B high performance gas chromatograph was used to analyze the product, and the internal standard method was used for quantification, with dodecane as the internal standard.
[0022] Conversion rate = (1-(amount of reactants after reaction / amount of reactants before reaction)) × 100%
[0023] Selectivity = (amount of tetrahydrofurfuryl alcohol / (amount of reactant before reaction - amount of reactant after reaction)) × 100%
[0024] Example 1
[0025] Using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O is uniformly loaded onto 1 gram of La2O3, and after aging and drying at 100°C in an oven for 24 hours, the catalyst precursor is ground. The catalyst precursor is placed in a tubular furnace, calcined at 400°C for 3 hours, cooled to 30°C, and then introduced with hydrogen with a purity of >99.99% at 400°C for 2 hours to obtain a Ni / La2O3 catalyst.
[0026] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0027] Example 2
[0028] Using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O is uniformly loaded onto 1 gram of La(OH)3, and then aged and dried in an oven at 100°C for 24 hours, and then ground to obtain a catalyst precursor. The catalyst precursor is placed in a tubular furnace, calcined at 500°C for 3 hours, cooled to 30°C, and then introduced with hydrogen with a purity of >99.99% at 400°C for 2 hours to obtain a Ni / La(OH)3 catalyst.
[0029] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0030] Example 3
[0031] By using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O is uniformly loaded onto 1 gram of La2O2CO3, and after aging and drying at 100°C in an oven for 24 hours, the catalyst precursor is ground. The catalyst precursor is placed in a tubular furnace, calcined at 500°C for 3 hours, cooled to 30°C, and then introduced with hydrogen with a purity of >99.99% at 400°C for 2 hours to obtain a Ni / La2O2CO3 catalyst.
[0032] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0033] Example 4
[0034] Using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O and 50 mg Fe(NO3)2·9H2O is uniformly loaded onto 1 gram of La2O2CO3, aged and dried in an oven at 100°C for 24 hours, and then ground to obtain a catalyst precursor. The catalyst precursor is placed in a tubular furnace, calcined at 500°C for 3 hours, cooled to 30°C, and then introduced with hydrogen with a purity of >99.99% at 400°C for 2 hours to obtain a Ni-Fe / La2O2CO3 catalyst.
[0035] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0036] Example 5
[0037] By using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O and 50 mg Fe(NO3)2·9H2O is uniformly loaded onto a mixed solid of 0.5 g La2O3 and 0.5 g La2O2CO3, and then aged and dried in an oven at 100°C for 24 hours, and then ground to obtain a catalyst precursor. The catalyst precursor is placed in a tubular furnace, calcined at 500°C for 3 hours, cooled to 30°C, and then introduced with hydrogen with a purity of >99.99% at 400°C for 2 hours to obtain a Ni-Fe / (La2O3+La2O2CO3) catalyst.
[0038] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0039] Example 6
[0040] By using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O and 50 mg RuCl3·3H2O is uniformly loaded onto 1 gram of La2O2CO3 mixed solid, and after aging and drying at 100°C in an oven for 24 hours, the catalyst precursor is ground. The catalyst precursor is placed in a tubular furnace, calcined at 500°C for 3 hours, cooled to 30°C, and then hydrogen with a purity of >99.99% is introduced at 400°C for 2 hours to obtain a NiRu / La2O2CO3 catalyst.
[0041] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0042] Example 7
[0043] By using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O, 50 mg RuCl3·3H2O and 50 mg Fe(NO3)2·9H2O is uniformly loaded onto 1 gram of La2O2CO3 mixed solid, aged and dried in an oven at 100°C for 24 hours, and then ground to obtain a catalyst precursor. The catalyst precursor is placed in a tubular furnace, calcined at 500°C for 3 hours, cooled to 30°C, and then hydrogen with a purity of >99.99% is introduced at 400°C for 2 hours to obtain a NiRu-Fe / La2O2CO3 catalyst.
[0044] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0045] Example 8
[0046] By using the equal volume impregnation method, an aqueous solution containing 500 mg Ni(NO3)2·6H2O, 50 mg RuCl3·3H2O, 50 mg Fe(NO3)2·9H2O and 50 mg Al(NO3)2·9H2O is uniformly loaded onto 1 gram of La2O2CO3 mixed solid, aged and dried in an oven at 100°C for 24 hours, and then ground to obtain a catalyst precursor. The catalyst precursor is placed in a tubular furnace, calcined at 500°C for 3 hours, cooled to 30°C, and then hydrogen with a purity of >99.99% is introduced at 400°C for 2 hours to obtain a NiRu-Fe-Al / La2O2CO3 catalyst.
[0047] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0048] Example 9
[0049] By using the equal volume impregnation method, an aqueous solution containing 50 mg of Fe(NO3)2·9H2O is uniformly loaded onto 1 gram of La2O2CO3, aged and dried in an oven at 100°C for 24 hours, ground, placed in a tube furnace, calcined at 500°C for 3 hours, cooled to 30°C, and obtained the catalyst precursor Fe / La2O2CO3. By using the equal volume impregnation method, an aqueous solution containing 500 mg of Ni(NO3)2·6H2O is uniformly loaded onto 1 gram of Fe / La2O2CO3, calcined at 500°C for 3 hours, cooled to 30°C, and introduced with hydrogen with a purity of >99.99% at 400°C for 2 hours to obtain a Fe-Ni / La2O2CO3 catalyst.
[0050] A fixed bed reactor was used, 1g of catalyst, ethanol as solvent, furfural concentration of 10mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20ml / min, hydrogen pressure of 1.5MPa, feed rate of 0.1mL / min, and after 8h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0051] Example 10
[0052] The catalyst of Example 6 was used in a fixed bed reactor, 1 g of catalyst, ethanol as solvent, furfural concentration of 10 mg / mL, reaction temperature of 120°C, hydrogen flow rate of 20 ml / min, hydrogen pressure of 1.5 MPa, feed rate of 0.1 mL / min, and after 200 h of reaction, the composition of the post-reaction solution was analyzed by gas chromatography. The conversion rate and selectivity are shown in Table 1.
[0053] Table 1. Conversion and selectivity results of furfural to tetrahydrofurfuryl alcohol catalyzed by examples 1-10
[0054]
[0055]
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing tetrahydrofurfuryl alcohol by hydrogenating furfural, characterized in that: Under the catalytic action of a catalyst, furfural and hydrogen are contacted and reacted to obtain tetrahydrofurfuryl alcohol; the catalyst comprises a carrier, an active metal and an auxiliary agent, wherein the carrier is at least one of La2O3, La(OH)3, and La2O2CO3, the active metal is at least one of Ni, Cu, and Pd, and the auxiliary agent is at least one of Ca, Mg, Sr, Ba, Cd, Fe, Ru, Zn, and Al.
2. The method according to claim 1, characterized in that The active metal accounts for 0.2-20% of the total mass of the catalyst, and the auxiliary agent accounts for 0-10% of the total mass of the catalyst.
3. The method according to claim 2, characterized in that The active metal accounts for 5-15% of the total mass of the catalyst, and the promoter accounts for 0.5-5% of the total mass of the catalyst.
4. The method according to claim 1, characterized in that: The preparation of the catalyst comprises the following steps: loading the active metal and the auxiliary agent onto the carrier by an impregnation method, and performing calcination and reduction treatment on the obtained solid in sequence after aging.
5. The method according to claim 4, characterized in that The aging temperature is 30-120°C, the aging time is 10-36h, the calcination temperature is 300-600°C, the calcination time is 1-5h, the reduction temperature is 300-500°C, and the reduction time is 1-5h.
6. The method according to claim 4, characterized in that The impregnation method is one of co-impregnation and two-step impregnation. The specific process of the co-impregnation is to impregnate the metal salt precursor solution containing the active metal and the metal salt precursor solution of the auxiliary agent onto the carrier; the specific process of the two-step impregnation is to first impregnate the metal salt precursor solution containing the active metal or the metal salt precursor solution containing the auxiliary agent onto the carrier, and then aging and calcining it, and then impregnating it with another solution, and then calcining and reducing it.
7. The method according to claim 6, characterized in that The metal salt precursor of the active metal is one or a combination of two or more of the nitrate, sulfate, chloride and acetate of the active metal, and the metal salt precursor of the auxiliary agent is one or a combination of two or more of the nitrate, sulfate, chloride and acetate of the auxiliary agent.
8. The method according to claim 1, characterized in that: The contact reaction is specifically carried out by passing hydrogen and a solution containing furfural into a fixed bed reactor, the reaction temperature is 50-200° C., the pressure of hydrogen is 0.5-6 MPa, and the liquid space velocity of the solution containing furfural is 0.1-2 h -1 , the molar ratio of hydrogen to furfural is (20-500):
1.
9. The method according to claim 8, characterized in that The reaction temperature is 80-140°C, the hydrogen pressure is 1-3MPa, and the liquid space velocity of the solution containing furfural is 0.3-0.8h -1 .
10. The method according to claim 8, characterized in that The solvent of the solution containing furfural is one or a mixed solvent of two or more of water, ethanol, methanol, isopropanol, 1,4-dioxane, tetrahydrofuran and acetonitrile.
Citation Information
Patent Citations
Method for preparing tetrahydrofurfuryl alcohol from furfural by aqueous phase hydrogenation
CN104672185A
Preparation method for tetrahydrofurfuryl alcohol
CN105693659A
Magnetic supported nickel catalyst as well as preparation method and application thereof