Normal-temperature self-crosslinking acrylate emulsion and preparation method thereof
A room temperature self-crosslinking acrylic emulsion with a three-dimensional network structure addresses the limitations of polyacrylate by enhancing water and weather resistance, enabling broader applications in coatings.
Patent Information
- Application Number
- CN202411307766.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-12-03
AI Technical Summary
Polyacrylate emulsion lacks cross-linking points, leading to issues such as hot stickiness, cold brittleness, poor weather resistance, and water resistance, limiting its application in coatings.
A room temperature self-crosslinking acrylic emulsion is prepared using 2-hydroxy-3-aminopropyl methacrylate solution, acrylic acid ester monomers, initiators, emulsifiers, buffers, and aldehyde solutions through a controlled polymerization process, forming a three-dimensional network structure.
The emulsion achieves high hardness, good water and weather resistance, and adhesion, expanding its application to water-based wood coatings, building anticorrosive coatings, and waterproof coatings with improved scrub resistance and resource efficiency.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of acrylic ester emulsion polymerization, and particularly relates to a room-temperature self-crosslinking emulsion and a preparation method thereof. Background Art
[0002] Water-based paint is safe and environmentally friendly, and is used to replace highly polluting solvent-based paint. Polyacrylate emulsion is a general name for various acrylic monomer copolymers. It has a wide range of monomer selection, low price, and mature process methods. The emulsion viscosity varies in a wide range and is highly controllable. It has good film-forming properties, adhesion, gloss and color retention, and stability. The various functional groups on the polymer can also react with other substances. It is easy to apply and change, and other advantages make it widely used in various industries, especially in the wood paint industry and the construction industry.
[0003] However, polyacrylate lacks cross-linking points between molecules, making it difficult to form a network structure, and has disadvantages such as hot stickiness and cold brittleness, poor weather resistance and water resistance, which greatly limits its application. The introduction of self-cross-linking monomers in emulsion polymerization increases the cross-linking density of the coating when the emulsion is cured to form a three-dimensional network structure, increases the hardness, adhesion and water resistance of the coating, improves the comprehensive performance of the emulsion after curing, expands the application field, and has a good application prospect. Summary of the invention
[0004] The purpose of the present invention is to provide a room temperature self-crosslinking acrylate emulsion and a preparation method thereof in view of the deficiencies in the prior art. The room temperature self-crosslinking acrylate emulsion of the present invention has good water resistance, weather resistance and mechanical strength, and the production method is simple and low in cost.
[0005] The room temperature self-crosslinking acrylic emulsion of the present invention has a formula composition of: 5-10 parts of 2-hydroxy-3-aminopropyl methacrylate solution, 40-70 parts of deionized water, 40-70 parts of acrylic acid ester monomers, 0.1-0.4 parts of initiator, 0.6-3 parts of emulsifier, 0.1-0.4 parts of buffer, and 1-10 parts of aldehyde solution;
[0006] The 2-hydroxy-3-aminopropyl methacrylate solution is prepared by adding glycidyl methacrylate and aqueous ammonia (25% content) in a weight ratio of 2:1 into a stirring kettle, heating the mixture to 60° C., and refluxing and stirring the mixture for three hours.
[0007] In the above-mentioned room temperature self-crosslinking acrylic emulsion, the acrylic ester monomer is one or more of methyl methacrylate, methyl acrylate, ethyl acrylate, styrene, butyl acrylate, butyl methacrylate, hydroxyethyl acrylate, isooctyl acrylate, and isobornyl acrylate.
[0008] In the above-mentioned room temperature self-crosslinking acrylic emulsion, the initiator is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.
[0009] In the above-mentioned room temperature self-crosslinking acrylic emulsion, the buffer is one or more of sodium dihydrogen phosphate, sodium bicarbonate, potassium dihydrogen phosphate, sodium acetate, and potassium bicarbonate.
[0010] The room temperature self-crosslinking acrylic emulsion mentioned above, the aldehyde solution is one or more of glyoxal aqueous solution, malondialdehyde aqueous solution, succinaldehyde aqueous solution, glutaraldehyde aqueous solution, o-phthalaldehyde aqueous solution.
[0011] The room temperature self-crosslinking acrylic emulsion mentioned above is prepared by mixing OP-10 and SDS (sodium dodecyl sulfate) in a weight ratio of 1:1 as the emulsifier.
[0012] The method for preparing a room temperature self-crosslinking acrylic emulsion comprises the following steps:
[0013] (1) preparing a 2-hydroxy-3-aminopropyl methacrylate solution: adding glycidyl methacrylate and aqueous ammonia (containing 25% by mass concentration of ammonia (NH3)) in a ratio of 2:1 to a stirred kettle, heating the kettle to 60° C., and refluxing and stirring for three hours to obtain a 2-hydroxy-3-aminopropyl methacrylate solution;
[0014] (2) adding part of deionized water, part of emulsifier, acrylic acid ester monomer, and 2-hydroxy-3-aminopropyl methacrylate aqueous solution into another stirring tank and stirring evenly to prepare a monomer pre-emulsion;
[0015] (3) preparing an initiator solution: stirring and dissolving an initiator in deionized water to prepare an initiator solution;
[0016] (4) Add the remaining deionized water, a small amount of initiator solution, the remaining emulsifier, the buffer, and part of the monomer pre-emulsion into the reactor, and raise the temperature to 80-85° C. at the same time, and react for 0.5 h. After no reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5 h, keep the temperature and react for 2 h, cool to room temperature, adjust the pH to neutral, add the aldehyde solution, and obtain a room temperature self-crosslinking acrylic emulsion after stirring and filtering.
[0017] The beneficial effects of the present invention are as follows: the acrylic emulsion prepared by the method of the present invention can undergo a cross-linking reaction at room temperature, and has a three-dimensional network structure, which greatly improves the cross-linking density of the coating film, has high hardness, good water resistance, acid and alkali resistance, adhesion and other properties, and has a simple process, low cost, and no need for heating and curing during film formation, which saves resources and greatly expands its application range. After testing, the water absorption rate is ≤3.5%, the weather resistance is ≥580h, and the scrub resistance is ≥4600. The one with better performance can reach a water absorption rate of ≤2.9%, a weather resistance of ≥640h, and a scrub resistance of ≥4700, and can be used for water-based wood coatings, building anticorrosive coatings, and waterproof coatings. DETAILED DESCRIPTION
[0018] The present invention is further described in detail below in conjunction with specific implementation modes.
[0019] Embodiment 1:
[0020] This embodiment provides a method for preparing a room temperature self-crosslinking acrylic emulsion, comprising the following steps:
[0021] 1. Weigh the following raw materials: 4 parts of glycidyl methacrylate, 2 parts of ammonia water (containing 25% mass percentage of ammonia (NH3)), 40 parts of deionized water, 20 parts of methyl methacrylate, 20 parts of butyl acrylate, 0.2 parts of potassium persulfate, 0.1 parts of sodium bicarbonate, 0.6 parts of emulsifier (OP-10: SDS (sodium dodecyl sulfate) mixed in a weight ratio of 1:1), and 5 parts of glyoxal solution.
[0022] 2. Prepare 2-hydroxy-3-aminopropyl methacrylate solution. Add glycidyl methacrylate and ammonia water into a stirring kettle, heat to 60°C, and reflux for three hours.
[0023] 3. In another stirred tank, add 35 parts of deionized water, 0.5 parts of emulsifier, methyl methacrylate, butyl acrylate, and the 2-hydroxy-3-aminopropyl methacrylate solution prepared in step 2 and stir evenly to prepare a monomer pre-emulsion.
[0024] 4. Prepare an initiator solution: Dissolve potassium persulfate in deionized water by stirring to prepare an initiator solution.
[0025] 5. Add 5 parts of deionized water, a small amount of initiator solution, 0.1 parts of emulsifier, sodium bicarbonate, and 8 parts of the monomer pre-emulsion prepared in step 3 into the reactor, and stir and heat to 80-85°C. Stir and react for 0.5h. After there is no obvious reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5h. After the addition is completed, keep the temperature for 2h, cool to room temperature, adjust the pH to neutral, add glyoxal solution, stir and filter to obtain the product.
[0026] Embodiment 2:
[0027] This embodiment provides a method for preparing a room temperature self-crosslinking acrylic emulsion, comprising the following steps:
[0028] 1. Weigh the following raw materials: 5 parts of glycidyl methacrylate, 2.5 parts of ammonia water (25% content), 40 parts of deionized water, 20 parts of methyl acrylate, 20 parts of butyl acrylate, 0.2 parts of potassium persulfate, 0.2 parts of sodium bicarbonate, 0.6 parts of emulsifier (OP-10: SDS mixed in a weight ratio of 1:1), and 10 parts of malondialdehyde solution.
[0029] 2. Preparation. Glycidyl methacrylate and ammonia water were added to a stirred kettle, heated to 60°C, and refluxed for three hours to obtain a 2-hydroxy-3-aminopropyl methacrylate solution.
[0030] 3. In another stirred tank, add 35 parts of deionized water, 0.5 parts of emulsifier, methyl acrylate, the 2-hydroxy-3-aminopropyl methacrylate solution prepared in step 2, and butyl acrylate, and stir evenly to prepare a monomer pre-emulsion.
[0031] 4. Prepare an initiator solution: Dissolve potassium persulfate in deionized water by stirring to prepare an initiator solution.
[0032] 5. Add 5 parts of deionized water, a small amount of initiator solution, 0.1 parts of emulsifier, sodium bicarbonate, and 8 parts of the monomer pre-emulsion prepared in step 3 into the reactor, and stir and heat to 80-85°C. Stir and react for 0.5h. After there is no obvious reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5h. After the addition is completed, keep the temperature for 2h, cool to room temperature, adjust the pH to neutral, add malondialdehyde solution, stir and filter to obtain the product.
[0033] Embodiment 3:
[0034] This embodiment provides a method for preparing a room temperature self-crosslinking acrylic emulsion, comprising the following steps:
[0035] 1. Weigh the following raw materials: 6 parts of glycidyl methacrylate, 3 parts of ammonia water (25% content), 60 parts of deionized water, 25 parts of styrene, 40 parts of isooctyl acrylate, 0.3 parts of sodium persulfate, 0.2 parts of potassium bicarbonate, 1.5 parts of emulsifier (OP-10: SDS mixed in a weight ratio of 1:1), and 7 parts of glutaraldehyde solution.
[0036] 2. Prepare 2-hydroxy-3-aminopropyl methacrylate solution. Add glycidyl methacrylate and ammonia water into a stirring kettle, heat to 60°C, and reflux for three hours.
[0037] 3. In another stirred tank, add 50 parts of deionized water, 1 part of emulsifier, styrene, the 2-hydroxy-3-aminopropyl methacrylate solution prepared in step 2, and isooctyl acrylate and stir evenly to prepare a monomer pre-emulsion.
[0038] 4. Prepare initiator solution: Dissolve sodium persulfate in deionized water by stirring to obtain an initiator solution.
[0039] 5. Add 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, potassium bicarbonate, and 10 parts of the monomer pre-emulsion prepared in step 3 into the reactor, and stir and heat to 80-85°C. Stir and react for 0.5h. After there is no obvious reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5h. After the addition is completed, keep the temperature for 2h, cool to room temperature, adjust the pH to neutral, add glutaraldehyde solution, stir and filter to obtain the product.
[0040] Embodiment 4:
[0041] This embodiment provides a method for preparing a room temperature self-crosslinking acrylic emulsion, comprising the following steps:
[0042] 1. Weigh the following raw materials: 4.6 parts of glycidyl methacrylate, 2.3 parts of ammonia water (25% content), 60 parts of deionized water, 25 parts of isobornyl acrylate, 40 parts of isooctyl acrylate, 0.3 parts of sodium persulfate, 0.2 parts of sodium acetate, 1.5 parts of emulsifier (OP-10: SDS mixed in a weight ratio of 1:1), and 8 parts of succinaldehyde solution.
[0043] 2. Prepare 2-hydroxy-3-aminopropyl methacrylate solution. Add glycidyl methacrylate and ammonia water into a stirring kettle, heat to 60°C, and reflux for three hours.
[0044] 3. In another stirred tank, add 50 parts of deionized water, 1 part of emulsifier, isobornyl acrylate, the 2-hydroxy-3-aminopropyl methacrylate solution prepared in step 2, and isooctyl acrylate and stir evenly to prepare a monomer pre-emulsion.
[0045] 4. Prepare initiator solution: Dissolve sodium persulfate in deionized water by stirring to obtain an initiator solution.
[0046] 5. Add 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, sodium acetate, and 7 parts of the monomer pre-emulsion prepared in step 3 into the reactor, and stir and heat to 80-85°C. Stir and react for 0.5 hours. After there is no obvious reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5 hours. After the addition is completed, keep the temperature for 2 hours, cool to room temperature, adjust the pH to neutral, add succinaldehyde solution, stir and filter to obtain the product.
[0047] Embodiment 5:
[0048] This embodiment provides a method for preparing a room temperature self-crosslinking acrylic emulsion, comprising the following steps:
[0049] 1. Weigh the following raw materials: 5.4 parts of glycidyl methacrylate, 2.7 parts of ammonia water (25% content), 60 parts of deionized water, 25 parts of isobornyl acrylate, 40 parts of isooctyl acrylate, 0.3 parts of sodium persulfate, 0.2 parts of sodium acetate, 1.5 parts of emulsifier (OP-10: SDS mixed in a weight ratio of 1:1), and 10 parts of o-phthalaldehyde solution.
[0050] 2. Prepare 2-hydroxy-3-aminopropyl methacrylate solution. Add glycidyl methacrylate and ammonia water into a stirring kettle, heat to 60°C, and reflux for three hours.
[0051] 3. In another stirred tank, add 50 parts of deionized water, 1 part of emulsifier, isobornyl acrylate, the 2-hydroxy-3-aminopropyl methacrylate solution prepared in step 2, and isooctyl acrylate and stir evenly to prepare a monomer pre-emulsion.
[0052] 4. Prepare an initiator solution: Dissolve sodium persulfate in deionized water by stirring to prepare an initiator solution.
[0053] 5. Add 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, sodium acetate, and 7 parts of the monomer pre-emulsion prepared in step 3 into the reactor, and stir and heat to 80-85°C. Stir and react for 0.5 hours. After there is no obvious reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5 hours. After the addition is complete, keep the temperature for 2 hours, cool to room temperature, adjust the pH to neutral, add o-phthalaldehyde solution, and obtain the product after stirring and filtering.
[0054] Embodiment 6:
[0055] This embodiment provides a method for preparing a room temperature self-crosslinking acrylic emulsion, comprising the following steps:
[0056] 1. Weigh the following raw materials: 6.2 parts of glycidyl methacrylate, 3.1 parts of ammonia water (25% content), 70 parts of deionized water, 15 parts of methyl acrylate, 15 parts of isobornyl acrylate, 40 parts of butyl acrylate, 0.4 parts of ammonium persulfate, 0.4 parts of sodium acetate, 3 parts of emulsifier (OP-10: SDS mixed in a weight ratio of 1:1), and 6 parts of succinaldehyde solution.
[0057] 2. Prepare 2-hydroxy-3-aminopropyl methacrylate solution. Add glycidyl methacrylate and ammonia water into a stirring kettle, heat to 60°C, and reflux for three hours.
[0058] 3. In another stirred tank, add 60 parts of deionized water, 2.5 parts of emulsifier, methyl acrylate, isobornyl acrylate, butyl acrylate, and the 2-hydroxy-3-aminopropyl methacrylate solution prepared in step 2, and stir evenly to prepare a monomer pre-emulsion.
[0059] 4. Prepare initiator solution: Dissolve ammonium persulfate in deionized water by stirring to prepare an initiator solution.
[0060] 5. Add 10 parts of deionized water, a small amount of initiator solution, 0.5 parts of emulsifier, sodium acetate, and 7 parts of the monomer pre-emulsion prepared in step 3 into the reactor, and stir and heat to 80-85°C. Stir and react for 0.5 hours. After there is no obvious reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5 hours. After the addition is completed, keep the temperature for 2 hours, cool to room temperature, adjust the pH to neutral, add succinaldehyde solution, stir and filter to obtain the product.
[0061] The finished products prepared in Examples 1-6 were subjected to various performance tests as shown in the following table, and the results are shown in the following table. The water absorption rate was tested according to the HG / T3344-2012 standard; the weather resistance was tested according to the GB / T 1865-2009 standard artificial aging test; and the scrub resistance was tested according to the GB / T 23989-2009 standard.
[0062] Water absorption Weather resistance Scrub resistance Example 1 3.1% 630h 4600 Example 2 3.0% 600h 4650 Example 3 2.8% 580h 4800 Example 4 2.9% 640h 4700 Example 5 3.4% 630h 4800 Example 6 3.5% 600h 4600
[0063] The present invention is a room temperature self-crosslinking acrylic emulsion and a preparation method thereof. The emulsion is obtained by free radical polymerization of the following components and weight parts of raw materials, wherein: 5-10 parts of 2-hydroxy-3-aminopropyl methacrylate solution, 40-70 parts of deionized water, 40-70 parts of acrylic ester monomers, 0.1-0.4 parts of initiators, 0.6-3 parts of emulsifiers, 0.1-0.4 parts of buffers, and 1-10 parts of aldehyde solutions. The preparation method thereof comprises the following steps: preparing 2-hydroxy-3-aminopropyl methacrylate solution, preparing monomer pre-emulsion liquid, and preparing initiator solution; adding deionized water, part of initiator solution, emulsifier, buffer solution, and part of monomer pre-emulsion liquid into a reactor, and heating the reactor to 80-85°C at the same time; after the preparation of the seed emulsion is completed, the remaining monomer pre-emulsion liquid and initiator solution are added dropwise; after the polymerization is completed, the temperature is lowered to room temperature, and the aldehyde solution is added to obtain the room temperature self-crosslinking acrylic emulsion.
[0064] As can be seen from the above table, the present invention has good water resistance, weather resistance, and scrub resistance, and can be used as water-based wood coatings, waterproof coatings, and building anticorrosive coatings.
Claims
1. A room temperature self-crosslinking acrylic emulsion, Its characteristics are: The formula composition is as follows by mass: 5-10 parts of 2-hydroxy-3-aminopropyl methacrylate solution, 40-70 parts of deionized water, 40-70 parts of acrylate monomer, 0.1-0.4 parts of initiator, 0.6-3 parts of emulsifier, 0.1-0.4 parts of buffer, and 1-10 parts of aldehyde solution; The 2-hydroxy-3-aminopropyl methacrylate solution is prepared by adding glycidyl methacrylate and aqueous ammonia (25% content) in a weight ratio of 2:1 into a stirring kettle, heating the mixture to 60° C., and refluxing and stirring the mixture for three hours.
2. The room temperature self-crosslinking acrylic emulsion according to claim 1, Features: The acrylic acid ester monomer is one or more of methyl methacrylate, methyl acrylate, ethyl acrylate, styrene, butyl acrylate, butyl methacrylate, hydroxyethyl acrylate, isooctyl acrylate and isobornyl acrylate.
3. The room temperature self-crosslinking acrylic emulsion according to claim 1, Features: The initiator is one or more of ammonium persulfate, potassium persulfate and sodium persulfate.
4. The room temperature self-crosslinking acrylic emulsion according to claim 1, Features: The buffer is one or more of sodium dihydrogen phosphate, sodium bicarbonate, potassium dihydrogen phosphate, sodium acetate and potassium bicarbonate.
5. The room temperature self-crosslinking acrylic emulsion according to claim 1, Features: The aldehyde solution is one or more of glyoxal aqueous solution, malondialdehyde aqueous solution, succinaldehyde aqueous solution, glutaraldehyde aqueous solution and o-phthalaldehyde aqueous solution.
6. The room temperature self-crosslinking acrylic emulsion according to claim 1, Features: The emulsifier is obtained by mixing OP-10 and SDS in a weight ratio of 1:
1.
7. The method for preparing the room temperature self-crosslinking acrylic emulsion according to claim 1, Its characteristics are: The following steps are involved: (1) Preparation of 2-hydroxy-3-aminopropyl methacrylate solution: Glycidyl methacrylate and aqueous ammonia are added into a stirred kettle, the temperature is raised to 60° C., and refluxed and stirred for three hours to obtain 2-hydroxy-3-aminopropyl methacrylate solution; (2) adding part of deionized water, part of emulsifier, acrylic acid ester monomer, and 2-hydroxy-3-aminopropyl methacrylate aqueous solution into another stirring tank and stirring evenly to prepare a monomer pre-emulsion; (3) preparing an initiator solution: stirring and dissolving an initiator in deionized water to prepare an initiator solution; (4) Add the remaining deionized water, a small amount of initiator solution, the remaining emulsifier, the buffer, and part of the monomer pre-emulsion into the reactor, and raise the temperature to 80-85° C. at the same time, and react for 0.5 h. After no reflux, slowly add the remaining monomer pre-emulsion and the remaining initiator solution dropwise within 1.5 h, keep the temperature and react for 2 h, cool to room temperature, adjust the pH to neutral, add the aldehyde solution, and obtain a room temperature self-crosslinking acrylic emulsion after stirring and filtering.