Resin composition and product thereof
A resin composition with benzoxazine resin and a pH-controlled compound addresses the limitations of existing copper clad laminates by enhancing dielectric properties and adhesion, resulting in improved PCB reliability and performance.
Patent Information
- Application Number
- CN202310625456.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
Existing copper clad laminates and resin compositions fail to meet the high requirements for advanced PCB packaging technology, including higher density, better electrical properties, and improved interconnect structure reliability, due to issues with dielectric loss aging rate, dielectric constant temperature coefficient, and resin-glass fiber adhesion.
A resin composition comprising benzoxazine resin with unsaturated carbon-carbon double bonds and a compound of formula (1) with a pH value of 5 to 10, prepolymerized to form a prepolymer, which is then combined with additional components like maleimide resin and fillers to enhance properties.
The resin composition achieves low dielectric loss aging rate, low dielectric constant temperature coefficient, high interlayer bond strength, and excellent resin-glass fiber adhesion, ensuring reliable PCB performance.
Smart Images

Figure CN119060262A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition and products made from the same, and in particular to a resin composition that can be used to prepare products such as prepregs, resin films, laminates or printed circuit boards. Background Art
[0002] As a basic electronic component, printed circuit boards (PCBs) are used in many fields including communications, industrial control, consumer electronics, automotive electronics, aerospace, etc. Their technical level has a direct impact on the technical stability and equipment reliability of electronic equipment. With the development of technologies such as 5G and the Internet of Things, the transmission rate and frequency of signals have been greatly improved. As the substrate material of PCB, copper clad laminate (CCL, or copper foil substrate) mainly plays the role of interconnection, insulation and support for PCB, and has a great influence on the transmission speed, energy loss, characteristic impedance and other aspects of the signal in the circuit. The characteristics, quality, processability in manufacturing, long-term reliability, stability and other characteristics of PCB depend to a large extent on the quality of copper clad laminate.
[0003] The problems of process capability, signal integrity, heat dissipation and stress currently faced by advanced PCB packaging technology have put forward higher requirements for the characteristics of copper clad laminates: higher density (such as high-density multilayer boards), better and more stable electrical properties (such as lower dielectric loss aging rate, lower dielectric constant temperature coefficient TcDk and dielectric loss temperature coefficient TcDf), etc. However, the existing copper clad laminates and the resin compositions used therein still mainly focus on the conventional characteristics of copper clad laminates.
[0004] Therefore, the art urgently needs to develop resin compositions and their copper-clad laminates and other products having excellent interconnect structure reliability, lower dielectric loss aging rate, lower dielectric constant temperature coefficient TcDk and dielectric loss temperature coefficient TcDf, while taking into account high-layer bonding strength, excellent filling properties, and resin and glass fiber interface adhesion. Summary of the invention
[0005] In view of the above-mentioned technical problems existing in the prior art, especially the problem that existing materials cannot meet one or more of the above-mentioned property requirements, the main purpose of the present invention is to provide a resin composition that can overcome at least one of the above-mentioned technical problems, and a product made of the resin composition.
[0006] The first aspect of the present invention provides a resin composition comprising the following components or prepolymers thereof:
[0007] (A) 100 parts by weight of a benzoxazine resin containing unsaturated carbon-carbon double bonds; and
[0008] (B) 10 to 50 parts by weight of a compound of formula (1), wherein the pH value of the compound of formula (1) is 5 to 10;
[0009]
[0010] In the formula (1), n is an integer of 3 to 6, X and Y are each independently an o-vinylphenoxy group or a p-vinylphenoxy group, and X and Y are not both o-vinylphenoxy and p-vinylphenoxy groups;
[0011] The prepolymer is obtained by prepolymerization of a mixture, and the mixture includes the component (A) and the component (B).
[0012] In one embodiment, for example, the prepolymer is formed by prepolymerization of the component (A) and the component (B), and the conversion rate of the prepolymerization is between 10% and 99%.
[0013] In one embodiment, for example, the benzoxazine resin containing unsaturated carbon-carbon double bonds includes any one of a modified benzoxazine resin of a compound containing unsaturated carbon-carbon double bonds, a bisphenol-type benzoxazine resin containing unsaturated carbon-carbon double bonds, a diamino-type benzoxazine resin containing unsaturated carbon-carbon double bonds, and a dicyclopentadiene-type benzoxazine resin containing unsaturated carbon-carbon double bonds, or a combination thereof.
[0014] In one embodiment, for example, the benzoxazine resin modified by the compound containing an unsaturated carbon-carbon double bond comprises a structure represented by formula (2):
[0015]
[0016] Among them, A is a covalent bond, -CH 2 -、-CH(CH 3 )- or -C(CH 3 ) 2 -; R 1 , R 2 , R 3 , R 4 are each independently hydrogen or a functional group containing an unsaturated carbon-carbon double bond, and R 1 , R 2 , R 3 , R 4 are not hydrogen at the same time; m is an integer from 1 to 10.
[0017] In one embodiment, for example, R 1 , R 2 , R 3 , R 4 Any one or combination of the following functional groups:
[0018]
[0019] Here, p is an integer from 0 to 25.
[0020] In one embodiment, for example, the bisphenol-type benzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure represented by formula (7):
[0021]
[0022] Among them, A 1 For covalent bonds, -CH 2 -、-CH(CH 3 )- or -C(CH 3 ) 2 -; R 7 , R 8 are each independently hydrogen or a C1-C3 alkyl group, a is each independently an integer from 0 to 3, R 5 , R 6 Each is independently a functional group containing an unsaturated carbon-carbon double bond.
[0023] In one embodiment, for example, the diaminobenzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure represented by formula (8):
[0024]
[0025] Among them, A 2 For covalent bonds, -O-, -CH 2 -、-CH(CH 3 )- or -C(CH 3 ) 2 -; R 9 , R 10 , R 12 , R 13 are each independently hydrogen or a C1-C3 alkyl group, b are each independently an integer from 0 to 3, e are each independently an integer from 0 to 4, R 11 , R 14 Each is independently a functional group containing an unsaturated carbon-carbon double bond.
[0026] In one embodiment, for example, the dicyclopentadiene-type benzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure represented by formula (9):
[0027]
[0028] Among them, R 17 , R 18 are each independently hydrogen or C1-C3 alkyl, R 15are each independently hydrogen, a C1-C3 alkyl group or an oxygen-containing functional group, q is an integer from 1 to 10, f is each independently an integer from 0 to 3, c is each independently an integer from 0 to 4, R 16 , R 19 Each is independently a functional group containing an unsaturated carbon-carbon double bond.
[0029] In one embodiment, for example, the resin composition further includes a maleimide resin, and the amount of the maleimide resin is 5 parts by weight to 20 parts by weight relative to 100 parts by weight of the benzoxazine resin containing an unsaturated carbon-carbon double bond.
[0030] In one embodiment, for example, the maleimide resin includes 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 3,3'-dimethyl-5,5'-dipropyl-4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, Any one of imide, 4-methyl-1,3-phenylene bismaleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, n-2,3-dimethylphenylmaleimide, n-2,6-dimethylphenylmaleimide, n-phenylmaleimide, vinylbenzylmaleimide, maleimide containing a biphenyl structure, maleimide containing an aliphatic structure of 10 to 50 carbon atoms, or a combination thereof.
[0031] In one embodiment, for example, the resin composition further comprises any one of a cross-linking agent containing unsaturated carbon-carbon double bonds, epoxy resin, polyester resin, phenol resin, amine curing agent, polyamide, polyimide, styrene maleic anhydride, and cyanate ester, or a combination thereof.
[0032] In one embodiment, for example, the resin composition further includes any one of an inorganic filler, a flame retardant, a hardening accelerator, an inhibitor, a solvent, a silane coupling agent, a colorant, and a toughening agent, or a combination thereof.
[0033] Another aspect of the present invention provides a product made of the above resin composition, wherein the product includes a prepreg, a resin film, a laminate or a printed circuit board.
[0034] In one embodiment, for example, the article has one or more of the following characteristics:
[0035] The resistance change rate after 1000 cycles measured by the interconnect stress test according to IPC-TM-650 2.6.26 is less than 10%;
[0036] After the product is left standing for 500 hours at a temperature of 85° C. and a relative humidity of 85%, the dielectric loss aging rate measured at a frequency of 10 GHz according to the method of JIS C2565 is less than or equal to 72%;
[0037] The interlayer bond strength measured according to IPC-TM-650 2.4.8 is greater than or equal to 4.6 lb / in;
[0038] The dielectric constant temperature coefficient measured according to IPC-TM-650 2.5.5.13 is less than or equal to 27ppm / ℃;
[0039] The dielectric loss temperature coefficient measured according to IPC-TM-650 2.5.5.13 is less than or equal to 5500ppm / ℃. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 An example diagram showing a shadow on the copper-free surface of an inner layer circuit substrate that does not contain copper in a glue filling test according to the present invention;
[0041] Figure 2 An example diagram showing that no shadow exists on the copper-free surface of the inner layer circuit substrate that does not contain copper in the glue filling test according to the present invention;
[0042] Figure 3 An example diagram showing a gap between the resin and the warp or weft glass fibers in the interface adhesion test according to the present invention;
[0043] Figure 4 An exemplary diagram showing that no gap exists between the resin and the glass fibers in the warp or weft direction in the interface adhesion test according to the present invention. DETAILED DESCRIPTION
[0044] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text have the common meanings understood by those skilled in the art for the present invention. In case of conflict, the definitions in this specification shall prevail.
[0045] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0046] The use of "one", "a", "an" or similar expressions to describe the components and technical features of the present invention is merely for the convenience of expression and to provide a general meaning to the scope of the present invention. Therefore, such description should be understood to include one or at least one, and the singular also includes the plural, unless it is obvious that it refers to another meaning.
[0047] As used herein, the terms "comprises," "includes," "has," "contains," or any other similar terms are open-ended transitional phrases, which are intended to cover non-exclusive inclusions. For example, a composition or article comprising a plurality of elements encompasses any one or any one of the listed elements, and is not limited to the elements listed herein, but may also include other elements that are not explicitly listed but are generally inherent to the composition or article. In addition, unless expressly stated to the contrary, the term "or" refers to an inclusive "or" rather than an exclusive "or." For example, any of the following situations satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist). In addition, in this article, the terms "comprising", "including", "having", and "containing" should be interpreted as being specifically disclosed and simultaneously covering closed conjunctions such as "consisting of", "consisting of", "the remainder of", and conjunctions such as "consisting essentially of", "mainly consisting of", "mainly consisting of", "basically containing", "essentially consisting of", "essentially consisting of", and "essentially containing".
[0048] As used herein, “or a combination thereof” means “or any combination thereof”, covering any combination of more than two of the listed elements; “any one”, “any one”, “any one” means “any one”, “any one”, “any one”. For example, “a composition or its product includes A, B, C or a combination thereof”, when interpreted, covers the following situations: A is true (or exists) and B and C are false (or do not exist), B is true (or exists) and A and C are false (or do not exist), C is true (or exists) and A and B are false (or do not exist), A and B are true (or exist) and C is false (or do not exist), A and C are true (or exist) and B is false (or do not exist), B and C are true (or exist) and A is false (or do not exist), A, B and C are all true (or exist), and other elements not explicitly listed but that are typically inherent to the composition or its product.
[0049] In this article, the terms "and", "with", "and", "as well as" or other similar terms are used to connect parallel sentence components, and there is no distinction between the previous and subsequent components. The meaning of the parallel sentence components does not change after the positions of the parallel sentence components are exchanged in grammatical sense.
[0050] In this article, all features or conditions such as numerical values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for simplicity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions), especially integer values. For example, the range description of "1.0 to 8.0", "between 1.0 and 8.0" or "between 1.0 to 8.0" should be deemed to have specifically disclosed all sub-ranges such as 1.0 to 8.0, 1.0 to 7.0, 2.0 to 8.0, 2.0 to 6.0, 3.0 to 6.0, 4.0 to 8.0, 3.0 to 8.0, etc., and should be deemed to cover endpoint values, especially sub-ranges defined by integer values, and should be deemed to have specifically disclosed individual values such as 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, etc. Unless otherwise indicated, the above explanation method applies to all contents of the entire text of the present invention, regardless of whether the scope is broad or not.
[0051] If the quantity, concentration or other numerical value or parameter is expressed as a range, a preferred range (or a better range) or a series of upper and lower limits, it should be understood that all ranges consisting of any pair of the upper limit or preferred value (or a better value) of the range and the lower limit or preferred value (or a better value) of the range have been specifically disclosed herein, regardless of whether these ranges are disclosed separately. In addition, if a numerical range is mentioned herein, unless otherwise specified, the range should include its endpoints and all integers and fractions within the range.
[0052] In this document, numerical values should be understood to have the accuracy of the number of significant digits of the numerical value, provided that the purpose of the invention can be achieved. For example, the number 40.0 should be understood to cover the range of 39.50 to 40.49.
[0053] In this document, when Markush groups or optional terms are used to describe features or embodiments of the present invention, those skilled in the art should understand that all subgroups or any individual elements in the Markush group or optional list can also be used to describe the present invention. For example, if X is described as "selected from X 1 , X 2 and X 3 ", which also means that X is fully described as X 1 The claim that X is X 1 and / or X 2 and / or X 3Furthermore, when Markush groups or optional terms are used to describe features or embodiments of the present invention, those skilled in the art will appreciate that any combination of subgroups or individual members of all elements in the Markush group or optional list can also be used to describe the present invention. Thus, for example, if X is described as "selected from X 1 , X 2 and X 3 and Y is described as "selected from the group consisting of Y 1 , Y 2 and Y 3 ", then it means that X has been fully described as X 1 and / or X 2 and / or X 3 And Y is Y 1 and / or Y 2 and / or Y 3 's claim.
[0054] Unless otherwise specified, in the present invention, a compound refers to a chemical substance formed by two or more elements connected by chemical bonds, including small molecule compounds and polymer compounds, but not limited thereto. The compound herein is not limited to a single chemical substance when interpreted, but can also be interpreted as the same type of chemical substances with the same composition or the same properties.
[0055] If not otherwise specified, in the present invention, polymer refers to the product formed by the polymerization reaction of monomers, often including many polymer aggregates, each polymer is composed of many simple structural units repeatedly connected by covalent bonds, and the monomer is a compound of the synthetic polymer. Polymers can include homopolymers, copolymers, prepolymers, etc., and are not limited to this. Homopolymers refer to polymers polymerized from one monomer. Copolymers refer to polymers polymerized from two or more monomers. Copolymers include random copolymers (structures such as -AABABBBAAABBA-), alternating copolymers (structures such as -ABABABAB-), graft copolymers (structures such as -AA(A-BBBB)AA(A-BBBB)AAA-) and block copolymers (structures such as -AAAAA-BBBBBB-AAAAA-), etc. For example, the styrene-butadiene copolymer in the present invention can include styrene-butadiene random copolymers, styrene-butadiene alternating copolymers, styrene-butadiene graft copolymers or styrene-butadiene block copolymers when interpreted. Prepolymer refers to a polymer with a lower molecular weight between the monomer and the final polymer, and the prepolymer contains reactive functional groups that can further undergo polymerization to obtain a fully cross-linked or hardened product with a higher molecular weight. Polymers of course include oligomers, but are not limited to them. Oligomers, also known as low polymers, are polymers composed of 2 to 20 repeating units, usually 2 to 5 repeating units.
[0056] For those skilled in the art, a resin composition containing three compounds A, B and C and an additive (comprising four components in total), and a resin composition containing a prepolymer formed by three compounds A, B and C and an additive (comprising two components in total) are different resin compositions, and the two are completely different in many aspects such as the preparation method, the physical and chemical properties of the compounds themselves, and the properties of their products. For example, the former is to mix A, B, C and additives to form a resin composition, while the latter is to first prepolymerize the mixture including A, B and C under appropriate conditions to form a prepolymer, and then mix the prepolymer with the additive to obtain a resin composition. For example, for those skilled in the art, the above two resin compositions have completely different compositions, and because the function of the prepolymer formed by the three compounds A, B and C in the resin composition is completely different from the function of A, B and C individually or together in the resin composition, the two resin compositions should be regarded as completely different chemical substances with completely different chemical positions. For example, for those skilled in the art, because the above two resin compositions are completely different chemical substances, their products will not have the same properties. For example, a resin composition including a prepolymer formed by three compounds A, B and C and a crosslinking agent, since A, B and C have partially reacted or converted during the prepolymerization reaction to form the prepolymer, when the resin composition is subsequently heated at a high temperature to form a semi-cured state, a partial crosslinking reaction occurs between the prepolymer and the crosslinking agent, rather than A, B and C each undergoing a partial crosslinking reaction with the crosslinking agent. Therefore, the products formed by the two resin compositions will also be completely different and have completely different properties.
[0057] If not otherwise specified, the "resin" in the present invention is a customary name for a synthetic polymer, which may include monomers, polymers thereof, combinations of monomers, combinations of polymers thereof, or combinations of monomers and polymers thereof, etc., and is not limited thereto.
[0058] If not otherwise specified, in the present invention, modified products include products after modification of reactive functional groups of each resin, products after prepolymerization of each resin with other resins, products after crosslinking of each resin with other resins, products after copolymerization of each resin with other resins, and the like.
[0059] If not otherwise specified, the unsaturated bond described in the present invention refers to a reactive unsaturated bond, such as an unsaturated double bond that can undergo a cross-linking reaction with other functional groups, such as an unsaturated carbon-carbon double bond that can undergo a cross-linking reaction with other functional groups.
[0060] The unsaturated carbon-carbon double bond described in the present invention preferably includes vinyl, vinylbenzyl, (meth)acryloyl, allyl or a combination thereof. Vinyl should be interpreted to include vinyl and vinylidene. (Meth)acryloyl should be interpreted to include acryloyl and methacryloyl.
[0061] Unless otherwise specified, the alkyl, alkenyl, and monomer described in the present invention include their various isomers when interpreted. For example, propyl should be interpreted as including n-propyl and isopropyl.
[0062] Unless otherwise specified, in the present invention, parts by weight represent relative parts by weight in the composition, and may be any weight unit, such as kilograms, grams, pounds, etc. For example, 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds may represent 100 kilograms of the benzoxazine resin containing unsaturated carbon-carbon double bonds or 100 pounds of the benzoxazine resin containing unsaturated carbon-carbon double bonds.
[0063] Unless otherwise specified, in the present invention, wt% represents weight (or mass) percentage.
[0064] It should be understood that the features disclosed in the various embodiments herein may be arbitrarily combined to form the technical solution of the present invention, as long as there is no contradiction in the combination of these features.
[0065] The present invention will be described below with specific embodiments and examples. It should be understood that these specific embodiments and examples are merely exemplary and are not intended to limit the scope of the present invention and its use. The methods, reagents and conditions used in the examples are, unless otherwise stated, methods, reagents and conditions conventional in the art.
[0066] The present invention discloses a resin composition, comprising the following components or prepolymers thereof:
[0067] (A) 100 parts by weight of a benzoxazine resin containing unsaturated carbon-carbon double bonds; and
[0068] (B) 10 to 50 parts by weight of a compound of formula (1), wherein the pH value of the compound of formula (1) is 5 to 10;
[0069]
[0070] In the formula (1), n is an integer of 3 to 6, X and Y are each independently an o-vinylphenoxy group or a p-vinylphenoxy group, and X and Y are not both o-vinylphenoxy and p-vinylphenoxy groups;
[0071] The prepolymer is obtained by prepolymerization of a mixture, and the mixture includes the component (A) and the component (B).
[0072] In one embodiment, for example, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention includes 10 to 50 parts by weight of the compound of formula (1) (whose pH value is 5 to 10), for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 30 parts by weight, 35 parts by weight, 40 parts by weight, 45 parts by weight or 50 parts by weight of the compound of formula (1) (whose pH value is 5 to 10).
[0073] Alternatively, in one embodiment, the resin composition comprises a prepolymer, which is formed by prepolymerization of 100 parts by weight of a benzoxazine resin containing unsaturated carbon-carbon double bonds as component (A) and 10 to 50 parts by weight of a compound of formula (1) (whose pH value is 5 to 10) as component (B). The prepolymer of the present invention contains residual unsaturated carbon-carbon double bonds, and the conversion rate of the reaction raw materials and the molecular weight of the prepolymer are both within a controllable range. In one embodiment, the residual unsaturated carbon-carbon double bonds in the prepolymer can react with other components (such as a cross-linking agent containing unsaturated carbon-carbon double bonds in the resin composition described herein), such as a polymerization reaction or a cross-linking reaction. In the present invention, the presence and content of the residual unsaturated carbon-carbon double bonds in the prepolymer are controlled by controlling the conversion rate of the compound of formula (1) and the benzoxazine resin containing unsaturated carbon-carbon double bonds. The conversion rate of the compound of formula (1) and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds is controlled by means known in the art, such as a hardening accelerator and / or a molecular weight regulator, as well as reaction temperature and reaction time.
[0074] In one embodiment, for example, the conversion rate of the prepolymerization reaction is between 10% and 99%, preferably between 30% and 95%, more preferably between 50% and 95%, particularly preferably between 50% and 90%, and most preferably between 75% and 90%. For example, when the conversion rate of the compound of formula (1) is 0%, it means that the compound of formula (1) is completely unreacted and the prepolymer of the present invention cannot be formed. When the conversion rate of the compound of formula (1) is 100%, it means that the compound of formula (1) is completely reacted, and the prepolymer of the present invention cannot be formed at this time.
[0075] For example, the prepolymer disclosed in the present invention can be prepared by the following method: a mixture comprising at least 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds and 10 to 50 parts by weight of the compound of formula (1) (with a pH value of 5 to 10) is subjected to a prepolymerization reaction under appropriate conditions.
[0076] For example, the above-mentioned prepolymerization reaction can be carried out in the presence of a hardening accelerator and / or a molecular weight regulator. The types of hardening accelerators are described in detail below. In one or more embodiments, the molecular weight regulator includes: n-butyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, mercaptoethanol, 2,4-diphenyl-4-methyl-1-pentene, 4,4'-butylenebis(6-tert-butyl-3-methylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof. The amount of the hardening accelerator and / or molecular weight regulator suitable for use in the present invention is not particularly limited, and relative to 100 parts by weight of the total amount of the benzoxazine resin containing unsaturated carbon-carbon double bonds and the compound of formula (1), each independently can be 0.01 to 5 parts by weight, for example, each independently 0.1 to 3 parts by weight, and is not limited thereto.
[0077] Typically, the benzoxazine resin containing unsaturated carbon-carbon double bonds and the compound of formula (1) (whose pH value is 5 to 10) and an optional hardening accelerator and / or a molecular weight regulator are dissolved in a solvent for prepolymerization. The solvent may be a solvent conventionally used in the art for polymerization between monomers or oligomers containing unsaturated carbon-carbon double bonds and benzoxazine resins containing unsaturated carbon-carbon double bonds, such as toluene and / or butanone. The temperature of the prepolymerization reaction is typically higher than room temperature, for example, between 50°C and 140°C, preferably between 70°C and 120°C. The reaction time is typically 4 to 16 hours, preferably 8 to 12 hours. The reaction is typically carried out under stirring conditions. Usually, before the reaction starts, the reaction temperature is first raised to above room temperature (about 25° C.). After a period of reaction, the temperature is lowered to room temperature to obtain a solution, and the solution is filtered using a filter to remove impurities. After the solution is purified, a prepolymer product is obtained, i.e., a prepolymer obtained by prepolymerizing the compound of formula (1) (whose pH value is 5 to 10) with a benzoxazine resin containing unsaturated carbon-carbon double bonds.
[0078] Examples of the benzoxazine resin containing unsaturated carbon-carbon double bonds are not particularly limited, and may include various benzoxazine resins known in the art that have at least one unsaturated carbon-carbon double bond in their molecular structures. These unsaturated carbon-carbon double bond reactive functional groups may undergo cross-linking reactions with other unsaturated bond-containing resins (e.g., maleimide resins) in the resin composition, thereby effectively improving the compatibility between the components and the heat resistance of the fully cured product.
[0079] In one embodiment, for example, examples of benzoxazine resins containing unsaturated carbon-carbon double bonds suitable for use in the present invention include any one of or a combination of benzoxazine resins modified with compounds containing unsaturated carbon-carbon double bonds, bisphenol-type benzoxazine resins containing unsaturated carbon-carbon double bonds, diamino-type benzoxazine resins containing unsaturated carbon-carbon double bonds, and dicyclopentadiene-type benzoxazine resins containing unsaturated carbon-carbon double bonds.
[0080] For example, the benzoxazine resin modified by the compound containing unsaturated carbon-carbon double bonds includes benzoxazine resin modified by olefin compounds, benzoxazine resin modified by acrylate compounds, benzoxazine resin modified by vinyl chloride compounds, or a combination thereof.
[0081] In one embodiment, for example, the benzoxazine resin modified by the compound containing an unsaturated carbon-carbon double bond comprises a structure represented by formula (2):
[0082]
[0083] Among them, A is a covalent bond, -CH 2 -、-CH(CH 3 )- or -C(CH 3 ) 2 -; R 1 , R 2 , R 3 , R 4 are each independently hydrogen or a functional group containing an unsaturated carbon-carbon double bond, and R 1 , R 2 , R 3 , R 4 are not hydrogen at the same time; m is an integer from 1 to 10.
[0084] Preferably, R 1 , R 2 , R 3 , R 4 Any one or combination of the following functional groups:
[0085]
[0086]
[0087] Here, p is an integer from 0 to 25.
[0088] In one embodiment, for example, the bisphenol-type benzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure represented by formula (7):
[0089]
[0090] Among them, A 1 For covalent bonds, -CH 2 -、-CH(CH 3 )- or -C(CH 3 ) 2 -; R 7 , R 8 are each independently hydrogen or a C1-C3 alkyl group, a is each independently an integer from 0 to 3, R 5 , R6 Each independently is a functional group containing an unsaturated carbon-carbon double bond. 5 , R 6 Each is independently a vinyl group, an allyl group, a vinylbenzyl group or a methacryloxy group.
[0091] In one embodiment, for example, the diaminobenzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure represented by formula (8):
[0092]
[0093] Among them, A 2 For covalent bonds, -O-, -CH 2 -、-CH(CH 3 )- or -C(CH 3 ) 2 -; R 9 , R 10 , R 12 , R 13 are each independently hydrogen or a C1-C3 alkyl group, b are each independently an integer from 0 to 3, e are each independently an integer from 0 to 4, R 11 , R 14 Each independently is a functional group containing an unsaturated carbon-carbon double bond. 11 , R 14 Each is independently a vinyl group, an allyl group, a vinylbenzyl group or a methacryloxy group.
[0094] In one embodiment, for example, the dicyclopentadiene-type benzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure represented by formula (9):
[0095]
[0096] Among them, R 17 , R 18 are each independently hydrogen or C1-C3 alkyl, R 15 are each independently hydrogen, a C1-C3 alkyl group or an oxygen-containing functional group, q is an integer from 1 to 10, f is each independently an integer from 0 to 3, c is each independently an integer from 0 to 4, R 16 , R 19 Each independently is a functional group containing an unsaturated carbon-carbon double bond. 16 , R 19 Each is independently a vinyl group, an allyl group, a vinylbenzyl group or a methacryloxy group.
[0097] In one embodiment, the benzoxazine resin containing unsaturated carbon-carbon double bonds suitable for the present invention can be any one or more commercial products, homemade products or combinations thereof. For example, commercial products can be purchased from Kolon and Huntsman, such as the trade name KZH-5031 sold by Kolon Industries of Korea.
[0098] In the present invention, the compound of formula (1) is a cyclic phosphazene compound containing a P=N bond in its structure, wherein n represents the number of P=N bonds, and n is an integer from 3 to 6. In other words, when n is 3, the compound of formula (1) has a six-membered ring cyclic phosphazene structure, and when n is 6, the compound of formula (1) has a twelve-membered ring cyclic phosphazene structure. In addition, the phosphorus atom in the cyclic phosphazene structure of the compound of formula (1) is substituted by an o-vinylphenoxy group or a p-vinylphenoxy group.
[0099] o-Vinylphenoxy: p-Vinylphenoxy:
[0100] In the present invention, for example, when n is 3, the number of o-vinylphenoxy groups in the cyclic phosphazene structure of the compound of formula (1) may be 1, 2, 3, 4 or 5, and the number of p-vinylphenoxy groups may be 5, 4, 3, 2 or 1. When n is 6, the number of o-vinylphenoxy groups in the cyclic phosphazene structure of the compound of formula (1) may be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or 11, and the number of p-vinylphenoxy groups may be 11, 10, 9, 8, 7, 6, 5, 4, 3, 2 or 1.
[0101] In the present invention, various compounds of formula (1) can be prepared by the methods described below, and the pH values of various compounds of formula (1) applicable to the present invention are 5 to 10. In the present invention, unless otherwise specified, the pH value of the compound can be measured by a measuring instrument known in the art, such as a pH meter, or titrated by acid-base titration. In one embodiment, for example, the compound of formula (1) and deionized water with a pH value of 7 are mixed in a weight ratio of 1:10, the mixed solution is filtered and extracted at room temperature, and the pH value of the extract is measured using a pH meter to obtain the pH value of the compound of formula (1). In one embodiment, for example, the pH value of the compound of formula (1) can be 5 to 10, for example, the pH value of the compound of formula (1) can be 5, 6, 7, 8, 9 or 10. When measured by a pH meter, the pH value of the compound of formula (1) can also be a small value, such as 5.5, 6.5 or 7.3, and is not limited thereto.
[0102] The compound of formula (1) of the present invention can be prepared by various methods known to those skilled in the art. For example, the compound of formula (1) can be prepared by the following method:
[0103] Step (1), reacting cyclophosphazene with o-hydroxybenzaldehyde to obtain an intermediate product 1;
[0104] Step (2), reacting the intermediate product 1 with p-hydroxybenzaldehyde to obtain the intermediate product 2;
[0105] Step (3), reacting the intermediate product 2 with methyltriphenylphosphonium bromide in the presence of a catalytic base to obtain a compound of formula (1).
[0106] In step (1), a base may be further added, including an acid binding agent, potassium carbonate, triethylamine or a combination thereof.
[0107] In step (1), an organic solvent may be further added, including tetrahydrofuran. Unless otherwise specified, the tetrahydrofuran used in the present invention is tetrahydrofuran from which water has been removed (anhydrous tetrahydrofuran).
[0108] In step (1), the cyclophosphazene includes hexachlorocyclotriphosphazene, octachlorocyclotetraphosphazene, decachlorocyclopentaphosphazene, and dodecachlorocyclohexaphosphazene. The molar ratio of the cyclophosphazene to o-hydroxybenzaldehyde is 1:1 to 1:11.
[0109] The reaction temperature of step (1) is 40 to 80° C., and the reaction time is 24 to 96 hours.
[0110] In step (2), the molar amount of p-hydroxybenzaldehyde added is 1 to 11 times the molar amount of cyclophosphazene added in step (1), that is, the molar ratio of cyclophosphazene to p-hydroxybenzaldehyde added is 1:1 to 1:11.
[0111] The reaction temperature of step (2) is 40 to 80° C., and the reaction time is 24 to 96 hours.
[0112] In step (3), an organic solvent from which water has been removed may be further added, including tetrahydrofuran from which water has been removed.
[0113] In step (3), the catalytic base includes potassium tert-butoxide, sodium methoxide or a combination thereof.
[0114] In step (3), the pH value of the reaction system is adjusted to 3 to 13 by using an acetic acid aqueous solution or an ammonium chloride aqueous solution.
[0115] The reaction temperature of step (3) is 25 to 50° C., and the reaction time is 1 to 6 hours.
[0116] In one embodiment, for example, the resin composition further comprises a maleimide resin, and the amount of the maleimide resin is not particularly limited, and can be 5 to 20 parts by weight, for example, 5 parts by weight, 10 parts by weight, 15 parts by weight, or 20 parts by weight, relative to 100 parts by weight of the benzoxazine resin containing an unsaturated carbon-carbon double bond.
[0117] The maleimide resin suitable for the resin composition of the present invention is not particularly limited, and can be any one or more maleimide resins suitable for making prepregs (or prepregs), resin films, laminates or printed circuit boards.
[0118] In one embodiment, the maleimide resin can be, for example, 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide (or oligomer of phenylmethane maleimide), bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 3,3'-dimethyl-5,5'-dipropyl ... any one of bismaleimide, m-phenylene bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, N-2,3-xylylmaleimide, N-2,6-xylylmaleimide, N-phenylmaleimide, vinyl benzyl maleimide (VBM), maleimide containing a biphenyl structure, and maleimide containing an aliphatic structure of 10 to 50 carbon atoms, or a combination thereof.
[0119] The term also includes modified products of these components, including diallyl compound modified maleimide resin, diamine modified maleimide resin, multifunctional amine modified maleimide resin, acidic phenol compound modified maleimide resin, cyanate modified maleimide resin or a combination thereof.
[0120] For example, the maleimide resins include maleimide resins produced by Daiwakasei Industry with trade names such as BMI-1000, BMI-1000H, BMI-1100, BMI-1100H, BMI-2000, BMI-2300, BMI-3000, BMI-3000H, BMI-4000, BMI-5000, BMI-5100, BMI-TMH, BMI-7000 and BMI-7000H, or maleimide resins produced by KI Chemical Co., Ltd. with trade names such as BMI-70 and BMI-80, or maleimide resins produced by Nippon Kayaku Co., Ltd. with trade names such as MIR-3000 and MIR-5000.
[0121] For example, maleimide resins with aliphatic structures containing 10 to 50 carbon atoms, or maleimide resins extended by imide, may include various maleimide resins extended by imide disclosed in Taiwan Patent Application Publication No. TW200508284A, which is incorporated herein by reference in its entirety. Maleimide resins with a structure containing 10 to 50 carbon atoms suitable for the present invention are, for example, maleimide resins produced by designer molecular companies under the trade names of BMI-689, BMI-1400, BMI-1500, BMI-1700, BMI-2500, BMI-3000, BMI-5000 and BMI-6000.
[0122] For example, if not otherwise specified, the cyanate-modified maleimide resin (or maleimide triazine resin) used in the present invention is not particularly limited, and can be any one or more maleimide triazine resins suitable for prepreg, resin film, laminate or printed circuit board production. For example, the maleimide triazine resin can be obtained by polymerizing a cyanate resin with the aforementioned maleimide resin. The maleimide triazine resin can be, for example, obtained by polymerizing a bisphenol A type cyanate resin with a maleimide resin, a bisphenol F type cyanate resin with a maleimide resin, a phenol novolac type cyanate resin with a maleimide resin, or a cyanate resin containing a dicyclopentadiene structure and a maleimide resin. For example, the maleimide triazine resin can be obtained by polymerizing a cyanate resin with a maleimide resin in any molar ratio. For example, the cyanate resin can be 1 to 10 moles relative to 1 mole of maleimide resin. For example, the cyanate resin is contained in an amount of 1, 2, 4 or 6 moles relative to 1 mole of the maleimide resin.
[0123] In one embodiment, for example, the resin composition may further include any one or a combination of a cross-linking agent containing unsaturated carbon-carbon double bonds, epoxy resin, polyester resin, phenol resin, amine curing agent, polyamide, polyimide, styrene maleic anhydride, and cyanate ester as needed.
[0124] In one embodiment, for example, the resin composition may further include a cross-linking agent containing unsaturated carbon-carbon double bonds. The resin composition of the present invention contains 1 to 20 parts by weight of the cross-linking agent containing unsaturated carbon-carbon double bonds relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds.
[0125] The cross-linking agent containing unsaturated carbon-carbon double bonds applicable to the present invention refers to a small molecule compound containing unsaturated carbon-carbon double bonds with a molecular weight less than or equal to 1000, and the molecular weight is preferably between 100 and 900, and more preferably between 100 and 800. For example, the cross-linking agent containing unsaturated carbon-carbon double bonds is any one of bis(vinylphenyl)ethane (BVPE), divinylbenzene (DVB), divinylnaphthalene, divinylbiphenyl, tert-butylstyrene, triallyl isocyanurate (TAIC), triallyl cyanurate (TAC), vinylbenzocyclobutene (VBCB), di(vinylbenzyl)ether (bis(vinylbenzyl)ether, BVBE), trivinylcyclohexane (TVCH), diallyl isophthalate (DAIP), diallyl bisphenol A (DABPA), acrylate, butadiene, decadiene, octadiene, vinyl carbazole, styrene, or a combination thereof.
[0126] In one embodiment, for example, the epoxy resin may be any epoxy resin known in the art. From the perspective of improving the heat resistance of the resin composition, the epoxy resin includes, for example, bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol AD epoxy resin, novolac epoxy resin, trifunctional epoxy resin, tetrafunctional epoxy resin, multifunctional novolac epoxy resin, dicyclopentadiene (DCPD) epoxy resin, phosphorus-containing epoxy resin, p-xylene epoxy resin, naphthalene epoxy resin (e.g., naphthol epoxy resin), benzofuran epoxy resin, isocyanate-modified epoxy resin, or a combination thereof. The novolac epoxy resin may be phenol novolac epoxy resin, bisphenol A novolac epoxy resin, bisphenol F novolac epoxy resin, biphenyl novolac epoxy resin, phenol benzaldehyde epoxy resin, phenol aralkyl novolac epoxy resin or o-cresol novolac epoxy resin; the phosphorus-containing epoxy resin may be DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) epoxy resin, DOPO-HQ epoxy resin or a combination thereof.The aforementioned DOPO epoxy resin may be selected from one or more of DOPO-containing phenolnovolac epoxy resin, DOPO-containing o-cresolnovolac epoxy resin and DOPO-containing bisphenol-Anovolac epoxy resin; the aforementioned DOPO-HQ epoxy resin may be selected from one or more of DOPO-HQ phenol novolac epoxy resin, DOPO-HQ-containing o-cresol novolac epoxy resin and DOPO-HQ bisphenol-A novolac epoxy resin.
[0127] Unless otherwise specified, the amount of the epoxy resin used in the present invention can be adjusted as needed. For example, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, the amount of the epoxy resin can be 10 to 100 parts by weight, such as 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, 80 parts by weight, 90 parts by weight or 100 parts by weight.
[0128] In one embodiment, for example, the polyester resin may be various polyester resins known in the art. Specific examples include polyester resins containing a dicyclopentadiene structure and polyester resins containing a naphthalene ring structure. Specific examples include the trade names HPC-8000 or HPC-8150 sold by Dainippon Ink Chemical. If not otherwise specified, the amount of the polyester resin used in the present invention can be adjusted as needed, for example, relative to 100 parts by weight of the benzoxazine resin containing an unsaturated carbon-carbon double bond, the amount of the polyester resin can be 10 to 80 parts by weight, such as 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight or 80 parts by weight.
[0129] In one embodiment, for example, the phenol resin may be various phenol resins known in the art, and specific examples include phenolic resins or phenoxy resins, wherein the phenolic resins include phenolic resins, o-methylphenolic resins, bisphenol A resins, naphthol resins, biphenyl resins, and dicyclopentadiene resins, and are not limited thereto. If not otherwise specified, the amount of the phenolic resin used in the present invention may be adjusted as needed, for example, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, the amount of the phenolic resin may be 10 to 80 parts by weight, for example, 10 parts by weight, 15 parts by weight, 20 parts by weight, 30 parts by weight, 40 parts by weight, 50 parts by weight, 60 parts by weight, 70 parts by weight, or 80 parts by weight.
[0130] In one embodiment, for example, the amine curing agent may be various amine curing agents known in the art. Specific examples include at least one of diaminodiphenyl sulfone, diaminodiphenylmethane, diaminodiphenyl ether, diaminodiphenyl sulfide and dicyandiamide or a combination thereof. If not otherwise specified, the amount of the amine curing agent used in the present invention can be adjusted as needed. For example, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, the amount of the amine curing agent can be 1 to 15 parts by weight, such as 1 part by weight, 4 parts by weight, 7.5 parts by weight, 12 parts by weight or 15 parts by weight.
[0131] In one embodiment, for example, the polyamide may be various polyamides known in the art, such as various commercially available polyamide resin products.
[0132] In one embodiment, for example, the polyimide may be various polyimides known in the art, such as various commercially available polyimide resin products.
[0133] In one embodiment, for example, the styrene maleic anhydride may be any type of styrene maleic anhydride known in the art, wherein the ratio of styrene (St) to maleic anhydride (MA) may be 1 / 1, 2 / 1, 3 / 1, 4 / 1, 6 / 1, 8 / 1 or 12 / 1. Specific examples include styrene maleic anhydride copolymers sold by Cray Valley under the trade names SMA-1000, SMA-2000, SMA-3000, EF-30, EF-40, EF-60 and EF-80, or styrene maleic anhydride copolymers sold by Polyscope under the trade names C400, C500, C700, C900, and the like, but are not limited thereto.
[0134] In one embodiment, for example, the cyanate ester may be any one or more cyanate ester resins suitable for use in the manufacture of prepregs, resin films, laminates or printed circuit boards. For example, a compound having an Ar-OC≡N structure, wherein Ar may be a substituted or unsubstituted aromatic group. From the perspective of improving the heat resistance of the resin composition, specific examples of cyanate ester resins include phenolic cyanate ester resins, bisphenol A cyanate ester resins, bisphenol F cyanate ester resins, cyanate ester resins containing dicyclopentadiene structures, cyanate ester resins containing naphthalene ring structures, phenolphthalein cyanate ester resins, adamantane cyanate ester resins, fluorene cyanate ester resins or combinations thereof. Among them, the phenolic cyanate ester resin may be a bisphenol A phenolic cyanate ester resin, a bisphenol F phenolic cyanate ester resin or a combination thereof. For example, the cyanate resin may be a cyanate resin produced by Lonza under the trade names of Primaset PT-15, PT-30S, PT-60S, BA-200, BA-230S, BA-3000S, BTP-2500, BTP-6020S, DT-4000, DT-7000, ULL950S, HTL-300, CE-320, LVT-50, LeCy, etc.
[0135] In addition to the aforementioned components, the resin composition of the present invention may further include an inorganic filler, a flame retardant, a hardening accelerator, an inhibitor, a solvent, a silane coupling agent, a colorant, a toughening agent or a combination thereof as needed.
[0136] In one embodiment, for example, the inorganic filler can be any one or more inorganic fillers suitable for the production of prepregs, resin films, laminates or printed circuit boards. Specific examples include: silicon dioxide (molten, non-molten, porous or hollow), aluminum oxide, aluminum hydroxide, magnesium oxide, magnesium hydroxide, calcium carbonate, aluminum nitride, boron nitride, aluminum silicon carbide, silicon carbide, titanium dioxide, barium titanate, lead titanate, strontium titanate, calcium titanate, magnesium titanate, barium zirconate, lead zirconate, magnesium zirconate, lead zirconate titanate, zinc molybdate, calcium molybdate, magnesium molybdate, ammonium molybdate, zinc molybdate modified talc, zinc oxide, zirconium oxide, mica, boehmite (boehmite, AlOOH), calcined talc, talc, silicon nitride, zirconium tungstate, petalite, calcined kaolin or a combination thereof. In addition, the inorganic filler may be spherical (including solid spherical or hollow spherical), fibrous, plate-like, granular, flake-like or needle-like, and may be selectively pretreated with a silane coupling agent. For example, in one embodiment, the resin composition of the present invention may further include 10 to 200 parts by weight of inorganic filler, preferably 50 to 150 parts by weight of inorganic filler, and more preferably 80 to 130 parts by weight of inorganic filler, relative to 100 parts by weight of benzoxazine resin containing unsaturated carbon-carbon double bonds, but is not limited thereto.
[0137] In one embodiment, for example, the flame retardant suitable for the present invention can be any one or more flame retardants suitable for the production of prepregs, resin films, laminates or printed circuit boards, such as phosphorus-containing flame retardants or bromine-containing flame retardants. The bromine-containing flame retardant preferably includes decabromodiphenylethane, and the phosphorus-containing flame retardant preferably includes: hydroquinone bis-(diphenyl phosphate), bisphenol A bis-(diphenyl phosphate), tri(2-carboxyethyl)phosphine (TCEP), tri(chloroisopropyl) phosphate, trimethyl phosphate (TMP), dimethyl methylphosphonate (DMMP), resorcinol bis(dixylenylphosphate), RDXP (such as commercial products such as PX-200, PX-201, PX-202), ammonium polyphosphate, melamine polyphosphate, etc. polyphosphate), DPPO (diphenylphosphineoxide) and its derivatives (such as bis-DPPO compounds) or resins, melamine cyanurate and tri-hydroxy ethyl isocyanurate, aluminum phosphinate (such as OP-930, OP-935 and other products) or combinations thereof.
[0138] In one embodiment, for example, the flame retardant can also be a flame retardant sold by Katayama Chemical Industry Co., Ltd., such as V1, V2, V3, V4, V5, V7, S-2, S-4, E-4c, E-7c, E-8g, E-9g, E-10g, E-100, B-3, W-1o, W-2h, W-2o, W-3o, W-4o, OX-1, OX-2, OX-4, OX-6, OX-6+, OX-7, OX-7+, OX-13, BPE-1, BPE-3, HyP-2, API-9, CMPO, ME-20, C-1R, C-1S, C-3R, C-3S or C-11R. The flame retardant of the present invention may include one or more of the above flame retardants.
[0139] In the present invention, the flame retardant is preferably a phosphate flame retardant, such as RDXP (such as commercially available products such as PX-200, PX-201, PX-202) and a flame retardant sold by Katayama Chemical Industry Co., Ltd. under the trade name S-2.
[0140] In one embodiment, for example, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 1 to 15 parts by weight of a phosphate flame retardant, preferably 4 to 10 parts by weight of a phosphate flame retardant, but not limited thereto.
[0141] The present invention preferably includes a phosphate flame retardant, such as but not limited to resorcinol bis-(xylyl phosphate) or its polycondensate, a phosphate containing an unsaturated carbon-carbon double bond, or a combination thereof.
[0142] The phosphate containing unsaturated carbon-carbon double bonds of the present invention includes the structure shown in P1,
[0143]
[0144] Wherein, A is independently a C1-C3 alkyl group, B is a functional group containing an unsaturated carbon-carbon double bond, preferably, B is vinyl, vinylbenzyl, allyl or butadienyl. Specific examples of the phosphate containing an unsaturated carbon-carbon double bond include, but are not limited to, flame retardants sold by Katayama Chemical Industry Co., Ltd. under the trade names of S-2, V2, and B-3.
[0145] In one embodiment, for example, the weight ratio of the compound of formula (1) to the phosphate flame retardant is between 6.25:1 and 1.5:1. For example, the weight ratio of the compound of formula (1) to the phosphate flame retardant is 6.25:1, 6:1, 5:1, 4:1, 3:1, 2.5:1, 2:1 or 1.5:1.
[0146] In one embodiment, for example, the hardening accelerator (including the hardening initiator) may include a catalyst such as a Lewis base or a Lewis acid. The Lewis base may include one or more of imidazole, boron trifluoride amine complex, ethyltriphenyl phosphonium chloride, 2-methylimidazole (2MI), 2-phenyl-1H-imidazole (2PZ), 2-ethyl-4-methylimidazole (2E4MI), triphenylphosphine (TPP) and 4-dimethylaminopyridine (DMAP). The Lewis acid may include a metal salt compound such as a metal salt compound of manganese, iron, cobalt, nickel, copper, zinc, etc., such as a metal catalyst such as zinc octoate and cobalt octoate. The hardening accelerator also includes a hardening initiator, such as a peroxide that can generate free radicals, and the hardening initiator includes: diisopropylbenzene peroxide, tert-butyl peroxybenzoate, dibenzoyl peroxide (BPO), 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne (25B) and bis(tert-butylperoxyisopropyl)benzene or a combination thereof. For example, in one embodiment, the resin composition of the present invention may further include 0.001 to 2 parts by weight of the hardening accelerator, preferably 0.01 to 1.5 parts by weight of the hardening accelerator, and more preferably 0.1 to 1.0 parts by weight of the hardening accelerator, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, but is not limited thereto.
[0147] In one embodiment, for example, the above-mentioned inhibitor may include 1,1-diphenyl-2-trinitrophenylhydrazine, methacrylonitrile, nitrogen oxide stable free radicals, triphenylmethyl free radicals, metal ion free radicals, sulfur free radicals (such as dithioesters), hydroquinone, p-methoxyphenol, p-benzoquinone, phenothiazine, β-phenylnaphthylamine, p-tert-butylcatechol, methylene blue, 4,4'-butylenebis(6-tert-butyl-3-methylphenol) and 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof. For example, the above-mentioned nitrogen oxide stable free radicals may include nitrogen oxide free radicals from cyclic hydroxylamines such as 2,2,6,6-tetramethyl-1-oxy-piperidine, 2,2,6,6-substituted-1-piperidinyloxy free radicals or 2,2,5,5-substituted-1-pyrrolidinyloxy free radicals. As a substituent, an alkyl group with a carbon number of less than four, such as a methyl group or an ethyl group, is preferred. Specific nitrogen oxide free radical compounds are not limited, and examples include 2,2,6,6-tetramethyl-1-piperidinyloxy free radicals, 2,2,6,6-tetraethyl-1-piperidinyloxy free radicals, 2,2,6,6-tetramethyl-4-oxo-1-piperidinyloxy free radicals, 2,2,5,5-tetramethyl-1-pyrrolidinyloxy free radicals, 1,1,3,3-tetramethyl-2-isoindolinyloxy free radicals, N,N-di-tert-butylamineoxy free radicals, etc. Stable free radicals such as galvinoxyl free radicals can also be used to replace nitrogen oxide free radicals. The inhibitor suitable for the resin composition of the present invention can also be a product derived from the hydrogen atom or atomic group in the inhibitor being replaced by other atoms or atomic groups. For example, the hydrogen atom in the inhibitor is replaced by an atomic group such as an amino group, a hydroxyl group, a ketocarbonyl group, and a derived product. For example, in one embodiment, the resin composition of the present invention may further include 0.001 to 20 parts by weight of a polymerization inhibitor, preferably 0.001 to 10 parts by weight of a polymerization inhibitor, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, but is not limited thereto.
[0148] In one embodiment, for example, the solvent suitable for the resin composition of the present invention is not particularly limited, and can be any solvent suitable for dissolving the resin composition of the present invention, including: methanol, ethanol, ethylene glycol monomethyl ether, acetone, butanone (also known as methyl ethyl ketone), methyl isobutyl ketone, cyclohexanone, nitrogen methyl pyrrolidone, toluene, xylene, methoxyethyl acetate, ethoxyethyl acetate, propoxyethyl acetate, ethyl acetate, dimethylformamide, dimethylacetamide, propylene glycol methyl ether acetate and other solvents or mixed solvents thereof. The amount of solvent added is to be able to completely dissolve the resin and adjust to a specific overall solid content of the resin composition. For example, in one embodiment, the amount of solvent added is adjusted to an overall solid content of the resin composition of 50% to 85% for addition, but is not limited thereto.
[0149] In one embodiment, for example, the silane coupling agent may include a silane compound (e.g., a siloxane compound), which may be further divided into amino silane compounds, epoxide silane compounds, vinyl silane compounds, hydroxy silane compounds, isocyanate silane compounds, methacryloxy silane compounds, and acryloxy silane compounds according to the type of functional group. For example, in one embodiment, the resin composition of the present invention may further include 0.001 to 20 parts by weight of a silane coupling agent, preferably 0.01 to 10 parts by weight of a silane coupling agent, relative to 100 parts by weight of a benzoxazine resin containing an unsaturated carbon-carbon double bond, but is not limited thereto.
[0150] In one embodiment, for example, the dye may include a dye or a pigment.
[0151] In the present invention, the main function of adding a toughening agent is to improve the toughness of the resin composition. In one embodiment, for example, the toughening agent may include carboxyl-terminated butadieneacrylonitrile rubber (CTBN), core-shell rubber, ethylene-propylene rubber and other compounds or combinations thereof. For example, in one embodiment, relative to 100 parts by weight of the benzoxazine resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 1 to 20 parts by weight of a toughening agent, preferably 3 to 10 parts by weight of a toughening agent, but is not limited thereto.
[0152] The aforementioned resin compositions can be made into various products, for example, components suitable for various electronic products, including prepregs, resin films, laminates or printed circuit boards.
[0153] For example, the resin composition of each embodiment of the present invention can be made into a semi-cured sheet, which includes a reinforcing material and a layered object arranged on the reinforcing material. The layered object is obtained by heating the aforementioned resin composition at a high temperature to form a semi-cured state (B-stage). The baking temperature for making the semi-cured sheet is between 120°C and 180°C, preferably between 120°C and 160°C. The reinforcing material can be any one of a fiber material, a woven fabric, and a non-woven fabric, and the woven fabric preferably includes a glass fiber cloth. The type of glass fiber cloth is not particularly limited, and can be various glass fiber cloths that can be used for printed circuit boards, such as E-type glass cloth, D-type glass cloth, S-type glass cloth, T-type glass cloth, L-type glass cloth, Q-type glass cloth or QL-type glass cloth (a glass cloth with a mixed structure made of Q glass and L glass). The types of glass fibers include yarns and rovings, etc., and the forms include open fiber or unopen fiber, and the end face shape includes a circular or flat shape. The aforementioned non-woven fabric preferably includes a liquid crystal resin non-woven fabric, such as a polyester non-woven fabric, a polyurethane non-woven fabric, etc., and is not limited thereto. The aforementioned fabric may also include a liquid crystal resin fabric, such as a polyester fabric or a polyurethane fabric, etc., and is not limited thereto. This reinforcing material can increase the mechanical strength of the prepreg. In a preferred embodiment, the reinforcing material can also be selectively pretreated with a silane coupling agent. The prepreg is subsequently heated and cured (C-stage) to form an insulating layer.
[0154] In one embodiment, for example, the resin composition of each embodiment of the present invention can be made into a resin film, which is obtained by semi-curing the aforementioned resin composition after baking and heating. The resin composition can be selectively coated on a liquid crystal resin film, a polytetrafluoroethylene film, a polyethylene terephthalate film (PET film), a polyimide film (PI film), a copper foil or a copper foil with adhesive, and then formed into a semi-cured state after baking and heating, so that the resin composition forms a resin film.
[0155] For example, the resin composition described in the present invention can be made into various laminates, which include at least two metal foils and at least one insulating layer, wherein the insulating layer is disposed between the two metal foils, and the insulating layer can be formed by curing the aforementioned resin composition under high temperature and high pressure (C-stage), and the applicable curing temperature is, for example, between 190°C and 220°C, preferably between 200°C and 210°C, and the curing time is 90 to 180 minutes, preferably 120 to 150 minutes. The aforementioned insulating layer can be obtained by curing the aforementioned semi-cured sheet or resin film. The material of the aforementioned metal foil can be copper, aluminum, nickel, platinum, silver, gold or their alloys, such as copper foil. In a preferred embodiment, the laminate is a copper foil substrate.
[0156] In one embodiment, the aforementioned laminate can be further processed into a printed circuit board.
[0157] One of the methods for making the printed circuit board of the present invention can be to use a double-sided copper-clad laminate (for example, product EM-827, which can be purchased from Taiwan Optoelectronics Materials Co., Ltd.) with a thickness of 28 mils and 1 ounce of HTE (High Temperature Elongation) copper foil, and then perform electroplating after drilling to form electrical conduction between the upper copper foil and the bottom copper foil. Then, the upper copper foil and the bottom copper foil are etched to form an inner layer circuit. Then, the inner layer circuit is browned and roughened to form a concave-convex structure on the surface to increase the roughness. Then, the copper foil, the aforementioned prepreg, the aforementioned inner layer circuit board, the aforementioned prepreg, and the copper foil are stacked in sequence, and then a vacuum laminating device is used to heat for 90 to 180 minutes at an environment of 190°C to 220°C to cure the insulating layer material of the prepreg. Then, various circuit board processing processes known in the art such as blackening, drilling, and copper plating are performed on the copper foil on the outermost surface to obtain a printed circuit board.
[0158] In one embodiment, the resin composition of the present invention and various products prepared therefrom have one or more of the following characteristics:
[0159] There is no shadow on the copper-free surface of the inner circuit substrate without copper on the surface;
[0160] The interface adhesion between the resin and the glass fiber in the substrate was observed to be qualified using a scanning electron microscope;
[0161] The resistance value change rate after 1000 cycles measured by the interconnect stress test according to IPC-TM-650 2.6.26 is less than 10% (the product passes the interconnect stress test);
[0162] After standing for 500 hours at a temperature of 85°C and a relative humidity of 85%, the dielectric loss aging rate calculated by the dielectric loss measured at a frequency of 10 GHz according to the method of JIS C2565 is less than or equal to 72%, preferably between 29% and 72%;
[0163] The interlayer bonding strength measured according to IPC-TM-650 2.4.8 is greater than or equal to 4.6 lb / in, preferably between 4.6 lb / in and 5.6 lb / in;
[0164] The dielectric constant temperature coefficient measured according to the method of IPC-TM-650 2.5.5.13 is less than or equal to 27ppm / °C, preferably between 14ppm / °C and 27ppm / °C; and
[0165] The dielectric loss temperature coefficient measured according to the method of IPC-TM-650 2.5.5.13 is less than or equal to 5500 ppm / °C, preferably between 2601 ppm / °C and 5500 ppm / °C.
[0166] Example
[0167] The resin compositions of the embodiments of the present invention and the comparative examples of the present invention were prepared using various raw materials from the following sources according to the amounts shown in Tables 1 to 4, and were further prepared into various test samples.
[0168] The chemical raw materials used in the embodiments of the present invention and the comparative examples are as follows:
[0169] Bz-1: polybutadiene modified benzoxazine resin, homemade.
[0170] Bz-2: Allyl-containing dicyclopentadiene-type benzoxazine resin, homemade.
[0171] Bz-3: Allyl-containing bisphenol A type benzoxazine resin, homemade.
[0172] BMI-5100: 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, purchased from Daiwakasei Industry.
[0173] BMI-2300: polyphenylmethane maleimide, available from Daiwakasei Industry.
[0174] BMI-3000: Maleimide with an aliphatic structure containing 10 to 50 carbon atoms, purchased from Designer Molecular Corporation.
[0175] Homemade compounds A1-A8 and C1-C6 are described in detail below.
[0176] SPV-100: Allylphosphazene, purchased from Otsuka Chemical.
[0177] Di-DOPO: di-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, the structural formula is shown in formula (10),
[0178]
[0179] PX-200: Resorcinol bis-(xylyl phosphate) (condensation polymer), or 1,3-phenylene phosphate tetrakis(2,6-dimethylphenyl) ester (condensation polymer), purchased from Daihachi Chemical Co., Ltd., Japan.
[0180] S-2: diethyl p-vinylbenzyl phosphate, purchased from Katayama Chemical Co., Ltd.
[0181] SC-2500SVJ: spherical silica with the surface treated with a silane coupling agent, purchased from Admatechs.
[0182] 25B: 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, purchased from NOF Corporation.
[0183] Solvent: A mixed solvent of dimethylacetamide and butanone in a weight ratio of 1:5, dimethylacetamide and butanone were purchased from Sinopec. The content of the solvent is expressed as "appropriate amount", which means that the content of the mixed solvent is adjusted to the overall solid content of the resin composition of 60% to 68% (solid content, S / C = 60% to 68%).
[0184] Homemade polybutadiene-modified benzoxazine resin Bz-1
[0185] 15 g of bisphenol A type benzoxazine resin and 0.229 g of aluminum chloride are added to a reaction device and dispersed in a dichloromethane solvent. The temperature is controlled at 50° C. to 60° C. and the reaction is continued with stirring for 1 to 2 hours to promote the ring opening of the bisphenol A type benzoxazine resin. Then 5 g of polybutadiene and 0.04 g of 1-methyl-3-n-butyl imidazole fluoroborate are added. Under a pressure of 0.5 to 0.8 MPa, the reaction temperature is controlled at 70 to 100° C. and the reaction is continued for 3 hours. After cooling and purification steps, a polybutadiene modified benzoxazine resin Bz-1 is obtained, the structural formula of which is shown in formula (11).
[0186]
[0187] Self-made dicyclopentadiene benzoxazine resin Bz-2 containing allyl group
[0188] At room temperature, 228 g (0.4 mol) of allylamine and 80 g (0.1 mol) of dicyclopentadiene phenol (PD-9110, purchased from Changchun Resin, number average molecular weight Mn=800 g / mol) were added to the reactor, and 240 g (0.8 mol, concentration of 10%) of formaldehyde aqueous solution was added dropwise. After the addition was completed, the temperature was raised to 90°C to 100°C for insulation reaction for 3 to 6 hours. After the reaction was completed, the water was separated and poured out, and the system was heated to 110 to 130°C until it was clear and transparent to obtain an allyl-containing dicyclopentadiene benzoxazine resin Bz-2, the structure of which is shown in formula (9), wherein, R 17 , R 18 is hydrogen, R 15 is a hydroxyl group, q is an integer from 1 to 10, f=3, c=1, R 16 , R 19 It is allyl.
[0189] Self-made Bisphenol A-type Benzoxazine Resin Bz-3 Containing Allyl Group
[0190] At room temperature, add 228 g (0.4 mol) of allylamine and 228 g (0.1 mol) of bisphenol A to the reactor, and drop 240 g (0.8 mol, concentration of 10%) of formaldehyde aqueous solution. After the dropwise addition is completed, heat to 90°C to 100°C and keep warm for 3 to 6 hours. After the reaction is completed, separate and pour out the water, heat the system to 110 to 130°C until it is clear and transparent, and obtain an allyl-containing bisphenol A type benzoxazine resin Bz-3, the structure of which is shown in formula (7), wherein A 1 -C(CH 3 ) 2 -;
[0191] R 7 , R 8 is hydrogen, a=3, R 5 , R 6 It is allyl.
[0192] Homemade diaminobenzoxazine resin Bz-4 containing allyl groups
[0193] At room temperature, 536 g (0.4 mol) of 2-allylphenol and 200 g (0.1 mol) of 4'4-diaminodiphenyl ether were added to the reactor, and 240 g (0.8 mol, concentration of 10%) of formaldehyde aqueous solution was added dropwise. After the addition was completed, the temperature was raised to 90°C to 100°C and kept for reaction for 3 to 6 hours. After the reaction was completed, the water was separated and poured out, and the system was heated to 110 to 130°C until it was clear and transparent to obtain an allyl-containing diaminobenzoxazine resin Bz-4, the structure of which is shown in formula (8), wherein A 2 -O-; R 9 , R 10 , R 12 , R 13 is hydrogen, b=3, e=4, R 11 , R 14 It is allyl.
[0194] Homemade compound A1:
[0195] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 37 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 40°C and the reaction was continued for 72 hours. Then, 366 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask, the reaction was continued for 48 hours, and the intermediate was obtained by filtering and rotary evaporation.
[0196] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 4.5 to 5, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquid was separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane:ethyl acetate=500:1-10:1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A1. The pH value was measured to be 5. The specific structure is shown in formula (12).
[0197]
[0198] If not otherwise specified, in the present invention, the pH value of the compound is determined as follows: the compound and deionized water with a pH value of 7 are mixed in a weight ratio of 1:10, the mixed solution is filtered and extracted at room temperature, and the pH value of the extract is determined by a pH meter to obtain the pH value of the compound.
[0199] Homemade compound A2:
[0200] At room temperature, 100 g of hexachlorocyclotriphosphazene, 198 g of triethylamine and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 110 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 50° C. and the reaction was continued for 64 hours. Then, 220 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 60 hours, filtered and rotary evaporated to obtain an intermediate.
[0201] At room temperature, 350 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquid was separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A2. The pH value was measured to be 8. The specific structure is shown in formula (13).
[0202]
[0203] Homemade compound A3:
[0204] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 183 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 60°C and the reaction was continued for 56 hours. Then, 73 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 72 hours, filtered and rotary evaporated to obtain an intermediate.
[0205] At room temperature, 400 g of dehydrated methyltriphenylphosphonium bromide and 550 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 48 g of freshly opened sodium methoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An aqueous ammonium chloride solution was added to adjust the pH value to 9 to 10, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane: ethyl acetate = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A3. The pH value was measured to be 10. The specific structure is shown in formula (14).
[0206]
[0207] Homemade compound A4:
[0208] At room temperature, 134 g of octachlorocyclotetraphosphazene, 359 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 147 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 70°C and the reaction was continued for 48 hours. Then, 293 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 48 hours, filtered and rotary evaporated to obtain an intermediate.
[0209] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of a dehydrated tetrahydrofuran solution of an intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 135 g of freshly unsealed potassium tert-butoxide were slowly added. After reacting for 3 hours, 700 g of calcium bromide were added, and the reaction was stirred for 48 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Dichloroethane was added, the liquids were separated, and the oil phase was collected. After the dichloroethane was removed by rotary evaporation, a mixed solution of cyclohexane and dichloroethane was used as a mobile phase (cyclohexane: dichloroethane = 500: 1-10: 1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A4. The pH value was measured to be 8, and the specific structure is shown in formula (15).
[0210]
[0211] Homemade compound A5:
[0212] At room temperature, 168 g of decachlorocyclopentaphosphazene, 442 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After fully dissolved, the three-necked flask was moved to an ice-water bath. 183 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 70°C and the reaction was continued for 48 hours. Then, 366 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 48 hours, filtered and rotary evaporated to obtain an intermediate.
[0213] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 170 g of freshly unsealed potassium tert-butoxide were slowly added. After reacting for 3 hours, 600 g of calcium bromide were added, and the reaction was stirred for 36 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane:ethyl acetate=500:1-10:1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A5. The pH value was measured to be 8, and the specific structure is shown in formula (16).
[0214]
[0215] Homemade compound A6:
[0216] At room temperature, 201 g of dodecachlorocyclohexaphosphazene, 525 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 220 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 70°C and the reaction was continued for 48 hours. Then, 440 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask, the reaction was continued for 60 hours, and the intermediate was obtained by filtration and rotary evaporation.
[0217] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide was slowly added. After reacting for 3 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 7 to 8, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane:ethyl acetate=500:1-10:1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A6. The pH value was measured to be 8, and the specific structure is shown in formula (17).
[0218]
[0219] Homemade compound A7:
[0220] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 110 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 40°C and the reaction was continued for 72 hours. Then, 220 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask, the reaction was continued for 48 hours, and the intermediate was obtained by filtering and rotary evaporation.
[0221] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 100 g of freshly unsealed potassium tert-butoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An acetic acid aqueous solution was added to adjust the pH value to 3 to 4, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane:ethyl acetate=500:1-10:1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A7. The pH value was measured to be 4, and the specific structure was shown in the aforementioned formula (13).
[0222] Homemade compound A8:
[0223] At room temperature, 100 g of hexachlorocyclotriphosphazene, 270 g of potassium carbonate and 400 ml of tetrahydrofuran were added to a three-necked flask. After sufficient dissolution, the three-necked flask was moved to an ice-water bath. 110 g of o-hydroxybenzaldehyde was slowly added dropwise to the three-necked flask. After 2 hours of dropwise addition, the temperature was raised to 60°C and the reaction was continued for 56 hours. Then, 220 ml of a tetrahydrofuran solution of p-hydroxybenzaldehyde with a concentration of 0.5 g / ml was added dropwise to the three-necked flask. The reaction was continued for 48 hours, filtered and rotary evaporated to obtain an intermediate.
[0224] At room temperature, 315 g of dehydrated methyltriphenylphosphonium bromide and 500 ml of dehydrated tetrahydrofuran solution of the intermediate with a concentration of 0.17 g / ml were added to a three-necked flask, stirred, and 48 g of freshly opened sodium methoxide was slowly added. After reacting for 2 hours, 600 g of calcium bromide was added, and the reaction was stirred for 24 hours. An aqueous ammonium chloride solution was added to adjust the pH value to 11 to 12, and tetrahydrofuran in the system was removed by rotary evaporation. Ethyl acetate was added, and the liquids were separated. The oil phase was collected. After the ethyl acetate was removed by rotary evaporation, a mixed solution of cyclohexane and ethyl acetate was used as a mobile phase (cyclohexane:ethyl acetate=500:1-10:1), and the product was separated and purified by a silica gel chromatography column to obtain a product labeled A8. The measured pH value was 11, and the specific structure was shown in the aforementioned formula (13).
[0225] Homemade compound C1:
[0226] 31.2 g of NaH and 400 ml of tetrahydrofuran were added to a 1-liter three-necked flask, nitrogen was introduced, the temperature was raised to 50°C with stirring, 97.7 g of o-hydroxybenzaldehyde was dissolved in 200 ml of tetrahydrofuran, and the mixture was slowly added dropwise to the three-necked flask. After the addition was completed, the reaction was continued for 4 hours. Then, 34.7 g of hexachlorocyclotriphosphazene was dissolved in 200 ml of tetrahydrofuran, added to the three-necked flask, the temperature was raised to 65°C, the reaction was carried out for 48 hours, centrifuged, filtered and dried several times to obtain an intermediate product.
[0227] Add dry methyltriphenylphosphine bromide (150% excess) and calcium hydride (150% excess) to tetrahydrofuran, and then add the intermediate product. After the reaction is complete, add acetic acid and stir for 1 hour. Filter with suction to obtain compound C1. The pH value is 8. The structure of compound C1 is shown in formula (18).
[0228]
[0229] Homemade compound C2:
[0230] 31.2 g of NaH and 400 ml of tetrahydrofuran were added to a 1-liter three-necked flask, nitrogen was introduced, and the temperature was stirred and raised to 50°C. 48.85 g of o-hydroxybenzaldehyde and 37.6 g of phenol were dissolved in 200 ml of tetrahydrofuran and slowly added dropwise to the three-necked flask. After the addition was completed, the reaction was continued for 4 hours. 34.7 g of hexachlorocyclotriphosphazene was dissolved in 200 ml of tetrahydrofuran, added to the three-necked flask, and the temperature was raised to 65°C for reaction for 48 hours. The intermediate product was obtained by centrifugation, filtration and drying for multiple times.
[0231] Add dry methyltriphenylphosphine bromide (150% excess) and calcium hydride (140% excess) to tetrahydrofuran, add the intermediate product, add acetic acid after the reaction is complete, stir for 1 hour, filter, and obtain compound C2. The pH value is 8. The structure of compound C2 is shown in formula (19).
[0232]
[0233] Homemade compound C3:
[0234] In a 5L four-necked flask equipped with a thermometer, a stirrer, a condenser, and a dropping funnel, a tetrahydrofuran (800 ml) solution of hexachlorocyclotriphosphazene (243.4 g, 2.10 mol) was added under a nitrogen stream, and a pre-prepared tetrahydrofuran (2000 ml) solution of sodium 4-acetylphenolate (797.0 g, 5.04 mol) was added dropwise thereto at 10 to 20° C. for 3.5 hours, and then stirred under reflux for 15 hours. After the reaction mixture was cooled to room temperature, the solvent was distilled off under reduced pressure, diluted with toluene (2000 ml), 5% aqueous sodium hydroxide solution (500 ml) was added and transferred to a separating funnel. After the water layer was separated, the toluene layer was washed with 5% aqueous sodium hydroxide solution (500 ml), and then neutralized with dilute nitric acid and washed with water. The toluene layer was concentrated under reduced pressure to obtain 642.19 g of an intermediate product, which was a cyclic phosphazene compound containing acetylphenoxy.
[0235] A solution of a cyclic phosphazene compound containing acetylphenoxy group (315.26 g, 1.00 mol) in tetrahydrofuran (3000 ml) was placed in a 5-liter autoclave under a nitrogen stream, and 10 wt% palladium-activated carbon (5.46 g) was added thereto. The autoclave was then pressurized with hydrogen and aged for 5 hours at room temperature. After confirming that the reaction was complete, Pd / C was filtered off, and tetrahydrofuran was removed by vacuum distillation to obtain 309.7 g of a product, which was compound C3, and the structure was shown in formula (20).
[0236]
[0237] Homemade compound C4:
[0238] With hexachlorocyclotriphosphazene, 3-vinylphenol and phenol as main raw materials, a p-vinylbenzene cyclotriphosphazene compound, i.e. compound C4, is synthesized by a stepwise addition method through a two-step nucleophilic substitution reaction. The structure is shown in formula (21).
[0239]
[0240] Homemade compound C5:
[0241] A solvent, hexachlorocyclotriphosphazene, vinylphenol (a mixture of p-vinylphenol and m-vinylphenol in a ratio of 50:50), and an acid-binding agent are added to a reaction apparatus, stirred, and nitrogen is introduced for protection. The reaction apparatus is heated to 50 to 120° C. A catalyst is then added to the reaction apparatus. The reaction is allowed to react for 5 to 16 hours, then cooled to room temperature, filtered, and the filtrate is subjected to pressure distillation to evaporate the solvent to obtain a brown powder or a viscous product, namely compound C5, whose structure is shown in formula (22).
[0242]
[0243] Homemade compound C6:
[0244] With 4-allyloxy-4'-hydroxydiphenyl sulfone and sodium as the main raw materials, tetrahydrofuran was added at 25°C for substitution reaction to obtain 4-allyloxy-4'-oxysodium diphenyl sulfone, and then an appropriate amount of hexachlorocyclotriphosphazene and tetrahydrofuran were added. After removing NaCl at 60°C, compound C6 was obtained. The structure is shown in formula (23).
[0245]
[0246] Preparation of prepolymer 1:
[0247] 100 parts by weight of Bz-1, 10 parts by weight of A2 and 110 parts by weight of butanone were added to a Schlenk reaction bottle, and after uniform dissolution, 0.9 parts by weight of VR-110 (azo initiator) was added. Vacuum was evacuated under a liquid nitrogen environment, and nitrogen was passed through. The above steps were repeated three times to discharge oxygen in the system. The temperature was raised to 75° C., and the reaction was carried out for 12 hours. After cooling, filtration and purification, a self-made prepolymer 1 was obtained, with a solid content of 100%, and the conversion rate of the self-made prepolymer 1 was between 10% and 99%.
[0248] Preparation of prepolymer 2:
[0249] 80 parts by weight of Bz-1, 50 parts by weight of A2, 20 parts by weight of Bz-2 and 150 parts by weight of butanone were added to a Schlenk reaction bottle, and after uniform dissolution, 1.3 parts by weight of VR-110 (azo initiator) was added. Vacuum was evacuated under a liquid nitrogen environment, and nitrogen was passed through. The above steps were repeated three times to discharge oxygen in the system. The temperature was raised to 80°C, and the reaction was carried out for 16 hours. After cooling, filtration and purification, a self-made prepolymer 2 was obtained, with a solid content of 100%, and the conversion rate of the self-made prepolymer 2 was between 10% and 99%.
[0250] The compositions of the resin compositions of the embodiments and comparative examples (all in parts by weight) and the test results of the properties are shown in Tables 1-4 below:
[0251] Table 1 Composition (unit: weight parts) and characteristic test results of the resin composition of the embodiment
[0252]
[0253]
[0254] Table 2 Composition (unit: weight parts) and characteristic test results of the resin composition of the embodiment
[0255]
[0256] Table 3 Composition (unit: weight parts) and characteristic test results of the resin composition of the comparative example
[0257]
[0258]
[0259] Table 4 Composition (unit: weight parts) and characteristic test results of the resin composition of the comparative example
[0260]
[0261]
[0262] In the present invention, the characteristic tests of the embodiments and comparative examples are performed by making the objects to be tested (samples) according to the following method and then performing the tests according to specific test conditions.
[0263] 1. Prepreg: The resin compositions in the embodiments or comparative examples are respectively selected and uniformly mixed to form a varnish, which is placed in an impregnation tank, and a glass fiber cloth (for example, L-glass fiber cloth (L-glass fiber fabric) with a specification of 2116, or L-glass fiber cloth (L-glass fiber fabric) with a specification of 1080, both purchased from Asahi Co., Ltd.) is immersed in the impregnation tank to adhere the resin composition to the glass fiber cloth, and heated at 150° C. to a semi-cured state (B-Stage) to obtain a prepreg.
[0264] 2. Copper foil substrate (8-ply, 8 prepregs pressed together): 2 ultra-low surface roughness (HVLP) copper foils with a thickness of 18 microns and 8 2116 L-glass fiber cloths were prepared to impregnate the prepregs made from each sample to be tested (each group of embodiments or comparative examples). The resin content of each prepreg was about 53%. One HVLP copper foil, eight prepregs and one HVLP copper foil were stacked in the order of one HVLP copper foil, eight prepregs and one HVLP copper foil, and pressed together for 2 hours under vacuum conditions, a pressure of 420 psi, and 200° C. to form a copper foil substrate. Among them, the 8 stacked prepregs were cured to form an insulating layer between the two copper foils, and the resin content of the insulating layer was about 53%.
[0265] 3. Copper-free substrate (8-ply, formed by pressing together 8 prepregs): The above copper foil substrate (8-ply) is etched to remove 2 copper foils to obtain a copper-free substrate (8-ply). The copper-free substrate is formed by pressing together 8 prepregs, and the resin content of the copper-free substrate is about 53%.
[0266] 4. Copper-free substrate (2-ply, formed by laminating two prepregs): prepare two ultra-low surface roughness (HVLP) copper foils with a thickness of 18 microns and two 1080 L-glass fiber cloths to impregnate the prepregs made from each sample to be tested (each group of embodiments or comparative examples), and stack them in the order of copper foil, two prepregs, and copper foil, and press them for 2 hours under vacuum conditions, a pressure of 420 psi, and 200° C. to form a copper-containing substrate (2-ply, formed by laminating two prepregs). Then, the copper-containing substrate (2-ply) is etched to remove the copper foil on both sides to obtain a copper-free substrate (2-ply), which is formed by laminating two prepregs, and the resin content of the copper-free substrate (2-ply) is about 70%.
[0267] For the above-mentioned samples to be tested, the test methods and their characteristic analysis items are described as follows:
[0268] 1. Filling
[0269] A 2.5 mil thick copper-containing substrate (e.g., product EM-827, available from Taiwan Optoelectronic Materials Co., Ltd.) was processed into a browned circuit board through a known browning process as the inner layer to evaluate the ability of the prepreg to flow and fill the empty areas between the circuits during lamination. The varnish of the resin composition of each group of embodiments or comparative examples was impregnated with 1017 L-glass fiber cloth, and baked at 140°C for 4 minutes to obtain a prepreg, and the resin content of the prepreg was about 79%. The 2.5 mil thick browned circuit board was laminated with a piece of the aforementioned prepreg (a prepreg obtained by impregnating 1017 L-glass fiber cloth with each sample to be tested (each group of embodiments or comparative examples)), and an ultra-low surface roughness copper foil (thickness of 18 microns) was laminated on the outer layer. In a vacuum press, it was pressed at 450psi and 210°C for 2 hours to form an inner layer circuit substrate with copper on the surface, and the outer layer copper foil was removed by etching to obtain an inner layer circuit substrate without copper on the surface. Repeat the above steps to make 15 inner circuit substrates without copper. Use an optical microscope to observe whether there is a shadow on the copper-free surface of the inner circuit substrate without copper. If there is a shadow on the surface, it means that the filling is poor, which will cause the subsequent circuit board to be scrapped. If at least one of the 15 inner circuit substrate samples without copper has a shadow on the surface (such as Figure 1If there is no shadow on the surface of the 15 inner circuit substrate samples without copper (such as Figure 2 As shown in the figure, it is marked as "pass", which means excellent filling performance.
[0270] 2. Interface adhesion
[0271] Select the aforementioned copper-free substrate (8-ply), cut a suitable size of glue-filled slices from the middle of the board, and use a Hitachi Regulus 8100 scanning electron microscope to observe whether there is a gap between the resin and the warp or weft glass fibers at a magnification of 10,000 times. If there is a gap, Figure 3 As shown, the mark "NG" means that the interface adhesion between the resin matrix and the glass fiber is poor and unqualified. Figure 4 As shown, it is marked as "pass", which means that the interface adhesion between the resin matrix and the glass fiber is excellent and qualified.
[0272] 3. Interconnect stress test (IST)
[0273] Interconnect stress test, also known as DC induction thermal cycle test, is a rapid method for thermal stress testing of finished PCB boards. It is used to evaluate the reliability of the interconnect structure (via) of the finished PCB.
[0274] According to the following structural description, the resin composition in the embodiment or comparative example is made into a 26-layer PCB board sample, dried, and then the PCB board sample is tested for the resistance value change rate after 1000 cycles of room temperature-150°C-room temperature (heating for 3 minutes, cooling for 2 minutes, 5 minutes as one cycle) using the interconnect stress test equipment model IST-HC produced by PWB Company, with reference to the method of IPC-TM-650 2.6.26. If the resistance value change rate is greater than or equal to 10%, it means unqualified, and it is marked as "NG", otherwise, if the resistance value change rate is less than 10%, it means qualified, and it is marked as "pass".
[0275] The structure design of the 26-layer PCB sample for interconnect stress testing is as follows:
[0276]
[0277]
[0278] Among them, 1oz copper foil corresponds to a thickness of 35 microns, Hoz copper foil corresponds to a copper foil thickness of 18 microns, and so on.
[0279] 4. Dielectric loss aging rate (Df aging rate)
[0280] The above copper-free substrate (2-ply) was measured with a microwave dielectrometer (purchased from AET, Japan) according to JIS C2565 method at room temperature (about 25°C) and at a frequency of 10 GHz. The dielectric loss value Df of each sample was measured and marked as Df 1 After the test, the sample was placed in a constant temperature and humidity chamber at 85°C and 85% relative humidity to absorb moisture for 500 hours, and the dielectric loss value Df was tested again, marked as Df 2 . Calculate using the formula: Df aging rate = ((Df after aging 2 -Df before aging 1 ) / Df before aging 1 )×100%.
[0281] 5. Bonding strength (B / S)
[0282] The copper foil substrate (made of eight prepregs pressed together) was cut into a rectangle with a width of 12.7 mm and a length greater than 60 mm, and measured using a universal tensile strength tester and referring to the method of IPC-TM-650 2.4.8. The surface copper foil does not need to be etched during the process, and the test position is the bonding surface between the second layer of prepreg and the third layer of prepreg. The force (lb / in) required to separate the two layers of the cured insulating substrate was tested at room temperature (about 25°C). The difference in interlayer bonding strength greater than 0.1 lb / in is considered to be significant.
[0283] 6. Temperature coefficient of dielectric constant (TcDk)
[0284] The aforementioned copper-free substrate (2-ply) was cut into square samples of 8 cm×8 cm, and the SPDR resonant cavity analyzer (split post dielectric resonant cavity, purchased from Waveray) was used to measure the change of the dielectric constant Dk of the sample at a frequency of 10 GHz and a relative humidity of 65%, and the temperature range of the sample was between 25°C and 150°C according to the method of IPC-TM-6502.5.5.13. The smaller the value of the dielectric constant temperature coefficient TcDk, the smaller the change value of the dielectric constant Dk when the temperature rises, which means that the dielectric constant of the insulation layer of the copper-free substrate is more stable, and the signal transmission of the subsequently manufactured printed circuit board in a high temperature environment is also more stable.
[0285] 7. Temperature coefficient of dielectric loss factor (TcDf)
[0286] The aforementioned copper-free substrate (2-ply) was cut into 8cm×8cm square samples, and the SPDR resonant cavity analyzer (split post dielectric resonant cavity, purchased from Waveray) was used to measure the change of the dielectric loss Df of the sample at a frequency of 10GHz and a relative humidity of 65%, and the temperature range of the sample was between 25°C and 150°C according to the method of IPC-TM-6502.5.5.13. The smaller the value of the dielectric loss temperature coefficient TcDf, the smaller the change value of the dielectric loss Df when the temperature rises, which means that the dielectric loss of the insulation layer of the copper-free substrate is more stable, and the signal integrity of the subsequently manufactured printed circuit board in a high temperature environment is better.
[0287] By referring to the test results in Tables 1 to 4, the following phenomena can be clearly observed.
[0288] By comparing Examples E1 to E8, E11 to E12 with Examples E9 to E10, it can be confirmed that the resin composition of the present invention, whether it is a technical solution comprising a benzoxazine resin containing an unsaturated carbon-carbon double bond and a compound of formula (1) (whose pH value is 5 to 10), or a technical solution comprising a prepolymer obtained by prepolymerizing a benzoxazine resin containing an unsaturated carbon-carbon double bond and a compound of formula (1) (whose pH value is 5 to 10), can also be improved in one or more aspects such as filling property, interface adhesion, interconnect stress test, dielectric loss aging rate, interlayer bonding strength, dielectric constant temperature coefficient TcDk, and dielectric loss temperature coefficient TcDf.
[0289] By comparing Examples E1, E2, and E4 with Comparative Examples C1 and C2, it can be found that if the amount of the compound of formula (1) is not in the range of 10 to 50 parts by weight, the filling properties, interface adhesion, interconnect stress test, and interlayer bonding strength are significantly reduced.
[0290] By observing the embodiments and comparative examples C3 and C4, it can be found that if the pH value of the compound of formula (1) is less than 5 or greater than 10, no significant improvement can be obtained in one or more aspects such as the filling property, interface adhesion, interconnect stress test, dielectric loss aging rate, interlayer bonding strength, dielectric constant temperature coefficient TcDk, and dielectric loss temperature coefficient TcDf.
[0291] By observing the embodiments and comparative examples C5 to C12, it can be found that if the compound of formula (1) (whose pH value is 5 to 10) is not used but only other compounds with a structure different from that of the compound of formula (1) are used, at least the interlayer bonding strength, dielectric constant temperature coefficient TcDk, dielectric loss temperature coefficient TcDf and other characteristics cannot be significantly improved.
[0292] Observing the embodiments E9-E10 using the prepolymer and other embodiments using the composition of the benzoxazine resin containing unsaturated carbon-carbon double bonds and the compound of formula (1) (whose pH value is 5 to 10), E9-E10 have lower dielectric loss aging rate and higher interlayer bonding strength.
[0293] The above embodiments are essentially only for auxiliary explanation and are not intended to limit the embodiments of the present invention or the application or use of these embodiments. In the present invention, words similar to "example" represent "as an example, example or illustration". Any illustrative embodiment herein is not necessarily interpreted as being preferred or more advantageous than other embodiments, unless otherwise specified.
[0294] In addition, although at least one exemplary embodiment or comparative example has been proposed in the aforementioned embodiments, it should be understood that the present invention may still have a large number of variations. It should also be understood that the embodiments described herein are not intended to limit the scope, use or configuration of the requested technical solution in any way. On the contrary, the aforementioned embodiments will provide a simple guide for those skilled in the art to implement one or more of the embodiments and their equivalents. Furthermore, the claims include known equivalents and all foreseeable equivalents when the present patent application is filed.
Claims
1. A resin composition, characterized in that Contains the following ingredients or their prepolymers: (A) 100 parts by weight of a benzoxazine resin containing unsaturated carbon-carbon double bonds; and (B) 10 to 50 parts by weight of a compound of formula (1), wherein the pH value of the compound of formula (1) is 5 to 10; In the formula (1), n is an integer of 3 to 6, X and Y are each independently an o-vinylphenoxy group or a p-vinylphenoxy group, and X and Y are not both o-vinylphenoxy and p-vinylphenoxy groups; The prepolymer is obtained by prepolymerization of a mixture, and the mixture includes the component (A) and the component (B).
2. The resin composition according to claim 1, characterized in that The prepolymer is formed by prepolymerization of the component (A) and the component (B), and the conversion rate of the prepolymerization is between 10% and 99%.
3. The resin composition according to claim 1, characterized in that The benzoxazine resin containing unsaturated carbon-carbon double bonds includes any one of a benzoxazine resin modified with a compound containing unsaturated carbon-carbon double bonds, a bisphenol-type benzoxazine resin containing unsaturated carbon-carbon double bonds, a diamino-type benzoxazine resin containing unsaturated carbon-carbon double bonds, and a dicyclopentadiene-type benzoxazine resin containing unsaturated carbon-carbon double bonds, or a combination thereof.
4. The resin composition according to claim 3, characterized in that The compound-modified benzoxazine resin containing an unsaturated carbon-carbon double bond comprises a structure shown in formula (2): Wherein, A is a covalent bond, -CH2-, -CH(CH3)- or -C(CH3)2-; R1, R2, R3, R4 are each independently hydrogen or a functional group containing an unsaturated carbon-carbon double bond, and R1, R2, R3, R4 are not hydrogen at the same time; m is an integer from 1 to 10.
5. The resin composition according to claim 4, characterized in that R1, R2, R3, R4 are selected from any one or a combination of the following functional groups: Here, p is an integer from 0 to 25.
6. The resin composition according to claim 3, characterized in that The bisphenol-type benzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure shown in formula (7): Wherein, A1 is a covalent bond, -CH2-, -CH(CH3)- or -C(CH3)2-; R7 and R8 are each independently hydrogen or a C1-C3 alkyl group, a is each independently an integer from 0 to 3, and R5 and R6 are each independently a functional group containing an unsaturated carbon-carbon double bond.
7. The resin composition according to claim 3, characterized in that The diaminobenzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure shown in formula (8): Wherein, A2 is a covalent bond, -O-, -CH2-, -CH(CH3)- or -C(CH3)2-; R9, R 10 , R 12 , R 13 are each independently hydrogen or a C1-C3 alkyl group, b are each independently an integer from 0 to 3, e are each independently an integer from 0 to 4, R 11 , R 14 Each is independently a functional group containing an unsaturated carbon-carbon double bond.
8. The resin composition according to claim 3, characterized in that The dicyclopentadiene-type benzoxazine resin containing unsaturated carbon-carbon double bonds comprises a structure shown in formula (9): Among them, R 17 , R 18 are each independently hydrogen or C1-C3 alkyl, R 15 are each independently hydrogen, a C1-C3 alkyl group or an oxygen-containing functional group, q is an integer from 1 to 10, f is each independently an integer from 0 to 3, c is each independently an integer from 0 to 4, R 16 , R 19 Each is independently a functional group containing an unsaturated carbon-carbon double bond.
9. The resin composition according to claim 1, characterized in that The resin composition further includes a maleimide resin, and the amount of the maleimide resin is 5 parts by weight to 20 parts by weight relative to 100 parts by weight of the benzoxazine resin containing an unsaturated carbon-carbon double bond.
10. The resin composition according to claim 9, characterized in that The maleimide resin includes any one of 4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 3,3'-dimethyl-5,5'-dipropyl-4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, n-2,3-dimethylphenylmaleimide, n-2,6-dimethylphenylmaleimide, n-phenylmaleimide, vinylbenzylmaleimide, maleimide containing biphenyl structure, and maleimide containing aliphatic structure of 10 to 50 carbon atoms, or a combination thereof.
11. The resin composition according to claim 1, characterized in that The resin composition further comprises any one of a crosslinking agent containing unsaturated carbon-carbon double bonds, epoxy resin, polyester resin, phenol resin, amine curing agent, polyamide, polyimide, styrene maleic anhydride, and cyanate ester, or a combination thereof.
12. The resin composition according to claim 1, characterized in that The resin composition further comprises any one of an inorganic filler, a flame retardant, a hardening accelerator, an inhibitor, a solvent, a silane coupling agent, a dye, and a toughening agent, or a combination thereof.
13. An article made of the resin composition according to any one of claims 1 to 12, characterized in that: The product includes a prepreg, a resin film, a laminate or a printed circuit board.
14. The product according to claim 13, characterized in that The product has one or more of the following characteristics: The resistance change rate after 1000 cycles measured by the interconnect stress test according to IPC-TM-650 2.6.26 is less than 10%; After the product is left to stand for 500 hours at a temperature of 85° C. and a relative humidity of 85%, the dielectric loss aging rate measured at a frequency of 10 GHz according to the method of JIS C2565 is less than or equal to 72%; The interlayer bond strength measured according to IPC-TM-650 2.4.8 is greater than or equal to 4.6 lb / in; The dielectric constant temperature coefficient measured according to IPC-TM-650 2.5.5.13 is less than or equal to 27ppm / ℃; The dielectric loss temperature coefficient measured according to IPC-TM-650 2.5.5.13 is less than or equal to 5500ppm / ℃.
Citation Information
Patent Citations
Imide-linked maleimide and polymaleimide compounds
TW200508284A
Cited By
Resin composition and product of the same
TWI939019B