Polymerization method of beta-butyrolactone

By using benzimidazole to replace aminophenoloxy zinc catalyst for polymerization of β-butyrolactone, the problem of insufficient activity and selectivity of existing catalysts was solved, and a high molecular weight and green environmentally friendly polymer was obtained, which was suitable for industrial applications.

CN119060314APending Publication Date: 2024-12-03EAST CHINA UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411217627.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing metal complex catalysts are difficult to take into account both catalytic activity, product molecular weight and stereoselectivity. The metals involved in catalysts with good performance are mainly rare earths, which are not economical and environmentally friendly enough, limiting the controllable ring-opening polymerization of β-butyrolactone. and copolymerization properties with multiple lactones.

Method used

The polymerization reaction of β-butyrolactone was carried out by benzimidazole instead of aminophenoloxy zinc catalyst, achieving high activity and high selectivity catalysis, obtaining β-butyrolactone polymer with high molecular weight, and performing one-pot copolymerization Generate random polymers.

Benefits of technology

The high activity and selectivity of the catalyst are achieved, and the obtained polymer has a higher molecular weight and a narrow molecular weight distribution, and the catalyst is more green and environmentally friendly, suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060314A_ABST
    Figure CN119060314A_ABST
Patent Text Reader

Abstract

The invention provides a polymerization method of beta-butyrolactone. The polymerization method comprises the following step: carrying out polymerization reaction on beta-butyrolactone and lactone under the catalysis condition of a benzimidazole substituted aminophenol oxygen group zinc catalyst. The aminophenol oxygroup zinc catalyst is a mononuclear zinc catalyst, and the structure of the aminophenol oxygroup zinc catalyst is shown as a formula (I). Compared with the prior art, the polymerization method provided by the invention has the advantages that beta-butyrolactone, lactide and epsilon-caprolactone are subjected to one-pot copolymerization with relatively high activity to obtain a polymer with high molecular weight, and synthesis of beta-butyrolactone copolymers with various chain structures is realized at the same time. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymers, in particular to a polymerization method of beta-butyrolactone. Background Art

[0002] The synthesis and application of plastics have brought a lot of convenience to people, but at the same time, they have also caused great harm to the environment and ecology. In recent years, with the deepening of the concept of sustainable development, in order to solve the problem of white pollution from the root, the development of biodegradable polymer materials has become the current trend, among which polyhydroxyalkanoates (PHA) are one of the bio-based materials that have received widespread attention.

[0003] Poly-3-hydroxybutyrate (P3HB) is the simplest and most studied polyhydroxyalkanoate. Poly-(R)-3-hydroxybutyrate (P-(R)-3HB) synthesized by microorganisms has an isotactic stereostructure and is a crystalline thermoplastic material. In terms of thermodynamics and physical properties, it is very close to isotactic polypropylene (i-PP) and is considered to be a biodegradable polymer material with comparable performance to isotactic polypropylene. However, the high cost of biofermentation synthesis of P3HB limits its market application. The use of chemical synthesis of P3HB can significantly reduce costs. Since the first report of the synthesis of P3HB by ring-opening polymerization of β-butyrolactone (β-BL) catalyzed by catalysts in 1961, the design and synthesis of catalysts with clear structures to achieve stereoselective catalytic polymerization of racemic β-butyrolactone (rac-β-BL) has become a research hotspot for the controllable synthesis of P3HB. However, to date, there are no other catalysts with both high activity and high isotactic stereoselectivity (P3HB) for rac-β-BL polymerization except rare earth complexes. m >0.85) of the catalysts reported.

[0004] In order to further develop new biodegradable polymer materials, the copolymerization of different monomers is expected to combine the advantages of different polymers and synthesize materials with better performance. In 2016, the Pappalardo research group reported that the aluminum complex of Salan ligand catalyzed the one-pot copolymerization of lactide (LA) and rac-β-BL. The polymerization rate of LA was much higher than that of rac-β-BL. After 2 hours of polymerization in toluene at 50°C, 88 equivalents of rac-LA were completely converted, while the same amount of rac-β-BL was converted by 66%. The alternating sequence of the obtained copolymer accounted for 35%, and the molecular weight M n =28kg / mol, which is larger than the theoretical value of 17kg / mol. w / M n=1.20 (New J. Chem., 2016, 40 (9), 7671-7679). In 2018, the Mazzeo research group reported that binuclear aluminum complexes were used to catalyze the copolymerization of rac-β-BL and ε-caprolactone. In toluene at 70°C, when ε-CL was converted to 70%, rac-β-BL began to polymerize. The molecular weight distribution of the copolymer obtained by catalysis was relatively wide, M w / M n =1.44; when rac-β-BL and L-LA are copolymerized, L-LA grows rapidly, while the polymerization of rac-β-BL monomer is not affected by LA, and the molecular weight distribution of the resulting polymer is narrow (Catal. Technol., 2018, 8(19), 5034-5043). In 2021, Dehghani's research group used stannous octoate to catalyze the one-pot copolymerization of ε-CL and rac-β-BL. The reaction was carried out at 110°C without solvent for 72 hours with a 1 mol% catalyst content. By controlling the ratio of the two monomers, three random copolymers P(HB-co-CL) with different ratios were prepared. Compared with P3HB, the tensile strength of the copolymer was not greatly affected, and the elongation at break and ductility were significantly improved (J. Appl. Poly. Sci., 2022, 139(22), e52240). In 2022, Yao Yingming's research group used binuclear rare earth complexes to catalyze the copolymerization of L-LA and rac-β-BL. A series of polymers were prepared by changing the monomer ratio. However, the LA monomer was first consumed to a very low concentration before rac-β-BL began to polymerize. When the rac-β-BL content in the copolymer increased, the glass transition temperature of the polymer showed a downward trend (Inorg. Chem., 2022, 61(26), 9918-9929).

[0005] As can be seen from the above, the controlled ring-opening polymerization of rac-β-BL and the preparation of new polymers by copolymerization with other lactones still face many technical problems. The metal complex catalysts reported so far are difficult to balance catalytic activity, product molecular weight and stereoselectivity, and the metals involved in the catalysts with better performance are mainly rare earths, which are not economical and environmentally friendly. Therefore, it is still necessary to develop efficient catalysts with good biocompatibility to achieve high activity and high selectivity in catalyzing the ring-opening polymerization of rac-β-BL and controllable copolymerization with a variety of lactone monomers to obtain new polyester polymers to meet the needs of industrial applications. Summary of the invention

[0006] The object of the present invention is to provide a polymerization method of β-butyrolactone.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a polymerization method of β-butyrolactone, comprising the following steps:

[0009] The β-butyrolactone and lactone are polymerized under the catalytic condition of benzimidazole-substituted aminophenoloxy zinc catalyst;

[0010] The benzimidazole-substituted aminophenoloxy zinc catalyst has a structure shown in formula (I):

[0011]

[0012] In the formula (I):

[0013] R 1 ~R 2 Represent hydrogen, C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 mono- or poly-aryl-substituted alkyl, halogen;

[0014] R 3 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 Mono- or poly-aryl-substituted alkyl, C6~C 18 The aromatic group;

[0015] R 4 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 A mono- or poly-aryl-substituted alkyl group;

[0016] X represents amino group NR 5 R 6 , where R 5 ~R 6 are C1-C6 straight chain, branched chain or cyclic alkyl, trimethylsilyl, triethylsilyl, dimethylhydrogensilyl, R 5 and R 6 Can be the same or different.

[0017] More specifically, in formula (I), R 1 ~R 2 are hydrogen, C1-C8 straight chain, branched chain or cyclic alkyl, C7-C 20 mono- or poly-aryl-substituted alkyl, halogen;

[0018] R 3 It is a C1-C8 straight chain, branched chain or cyclic alkyl group, C7-C 20 Mono- or poly-aryl-substituted alkyl, C6~C 12 The aromatic group;

[0019] R4 It is a C1-C8 straight chain, branched chain or cyclic alkyl group, C7-C 20 A mono- or poly-aryl-substituted alkyl group;

[0020] X represents trimethylsilyl, triethylsilyl, or dimethylhydrogensilyl.

[0021] Preferably, in formula (I), R 1 ~R 2 is methyl, tert-butyl, cumyl, trityl, chlorine;

[0022] R 3 is methyl, ethyl, isopropyl, n-butyl, tert-butyl, isopentyl, cyclohexyl, cyclopentyl, n-hexyl, n-octyl, benzyl, phenethyl, phenyl;

[0023] R 4 is methyl, ethyl, isopropyl, n-butyl, cyclohexyl, benzyl, phenethyl;

[0024] X is trimethylsilyl nitrogen group.

[0025] Preferably, the benzimidazole-substituted aminophenoloxy zinc catalyst shown in formula (I) has one of the following structures:

[0026]

[0027] Preferably, the molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to β-butyrolactone is 1:(50-10000).

[0028] The molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the lactone is 1:(0-10000).

[0029] More preferably, the molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to β-butyrolactone is 1:(50-5000).

[0030] The molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the lactone is 1:(0-5000).

[0031] Preferably, the β-butyrolactone is one or more of L-β-butyrolactone, D-β-butyrolactone, and rac-β-butyrolactone.

[0032] Preferably, the lactone is one or more of L-β-butyrolactone, D-β-butyrolactone, rac-β-butyrolactone, L-lactide, D-lactide, rac-lactide, meso-lactide, ε-caprolactone, γ-butyrolactone, and δ-valerolactone.

[0033] Preferably, the polymerization reaction temperature is -70 to 250°C;

[0034] The polymerization reaction is carried out under an inert atmosphere.

[0035] Preferably, the raw materials for the polymerization reaction further include alcohol compounds;

[0036] The molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the alcohol compound is 1:(0-20).

[0037] Preferably, the alcohol compound is C1 to C 10 Alkyl alcohols with straight chain, branched chain or cyclic structure, or C7~C 20 A mono- or poly-aryl-substituted alkyl alcohol.

[0038] The invention provides a polymerization method of beta-butyrolactone, comprising the following steps: subjecting beta-butyrolactone and lactone to polymerization reaction under the catalysis of a benzimidazole-substituted aminophenoloxy zinc catalyst.

[0039] Compared with the prior art, the polymerization method provided by the present invention enables the catalyst to have higher activity for the polymerization of β-butyrolactone, and simultaneously obtains a β-butyrolactone polymer with a high molecular weight; and realizes the one-pot copolymerization of β-butyrolactone with two or three monomers of lactide and ε-caprolactone. The results of the examples of the present application show that the copolymer obtained by the present invention is a single polymer. DETAILED DESCRIPTION

[0040] The present invention provides a polymerization method of β-butyrolactone, comprising the following steps:

[0041] The β-butyrolactone and lactone are polymerized under the catalytic condition of benzimidazole-substituted aminophenoloxy zinc catalyst;

[0042] The benzimidazole-substituted aminophenoloxy zinc catalyst has a structure shown in formula (I):

[0043]

[0044] In the formula (I):

[0045] R 1 ~R 2 Represent hydrogen, C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 mono- or poly-aryl-substituted alkyl, halogen;

[0046] R 3 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 Mono- or poly-aryl-substituted alkyl, C6~C 18 The aromatic group;

[0047] R 4 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 A mono- or poly-aryl-substituted alkyl group;

[0048] X represents amino group NR 5 R 6 , where R 5 ~R 6 are C1-C6 straight chain, branched chain or cyclic alkyl, trimethylsilyl, triethylsilyl, dimethylhydrogensilyl, R 5 and R 6 Can be the same or different.

[0049] More specifically, in formula (I), R 1 ~R 2 are hydrogen, C1-C8 straight chain, branched chain or cyclic alkyl, C7-C 20 mono- or poly-aryl-substituted alkyl, halogen;

[0050] R 3 It is a C1-C8 straight chain, branched chain or cyclic alkyl group, C7-C 20 Mono- or poly-aryl-substituted alkyl, C6~C 12 The aromatic group;

[0051] R 4 It is a C1-C8 straight chain, branched chain or cyclic alkyl group, C7-C 20 A mono- or poly-aryl-substituted alkyl group;

[0052] X represents trimethylsilyl, triethylsilyl, or dimethylhydrogensilyl.

[0053] Preferably, in formula (I), R 1 ~R 2 is methyl, tert-butyl, cumyl, trityl, chlorine;

[0054] R 3 is methyl, ethyl, isopropyl, n-butyl, tert-butyl, isopentyl, cyclohexyl, cyclopentyl, n-hexyl, n-octyl, benzyl, phenethyl, phenyl;

[0055] R 4 is methyl, ethyl, isopropyl, n-butyl, cyclohexyl, benzyl, phenethyl;

[0056] X is trimethylsilyl nitrogen group.

[0057] Preferably, the benzimidazole-substituted aminophenoloxy zinc catalyst shown in formula (I) has one of the following structures:

[0058]

[0059] The benzimidazole-substituted aminophenoloxy zinc catalyst shown in formula (I) of the present invention can be synthesized with reference to the method disclosed in patent CN202210076002.3, and its corresponding multi-dentate aminophenol ligand can be synthesized with reference to the method disclosed in patents ZL201910187042.3 and ZL200910197687.1.

[0060] The benzimidazole-substituted aminophenoloxy zinc catalyst of the present invention introduces metal zinc as a catalytic center, so that the complex is greener and more environmentally friendly than a large number of reported rare earth metal catalysts, and has a similar activity.

[0061] The present invention has no special restrictions on the sources of the benzimidazole-substituted aminophenol oxy zinc catalyst, β-butyrolactone and lactone. The benzimidazole-substituted aminophenol oxy zinc catalyst, β-butyrolactone and lactone well known to those skilled in the art can be used. Specifically, the benzimidazole-substituted aminophenol oxy zinc catalyst, β-butyrolactone and lactone can be commercially available products or homemade products. The present invention has no special restrictions on the homemade method of the benzimidazole-substituted aminophenol oxy zinc catalyst, β-butyrolactone and lactone. The benzimidazole-substituted aminophenol oxy zinc catalyst, β-butyrolactone and lactone in the present invention can be obtained. The present invention has no special requirements on the mixing order of the catalyst, β-butyrolactone and lactone. The catalyst, β-butyrolactone and lactone can be mixed in any order.

[0062] In the present invention, the molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to β-butyrolactone is preferably 1:(50-10000), more preferably 1:(50-5000), and most preferably 1:(100-1000).

[0063] In the present invention, the molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the lactone is preferably 1:(0-10000), more preferably 1:(0-5000), and most preferably 1:(0-1000).

[0064] The present invention has no special requirements for the molar ratio of the β-butyrolactone to the lactone, and the requirements of the molar ratio of the catalyst to the β-butyrolactone and the molar ratio of the catalyst to the lactone can be met. In the present invention, the molar ratio of the β-butyrolactone to the lactone can be any value.

[0065] In the present invention, the β-butyrolactone is preferably one or more of L-β-butyrolactone, D-β-butyrolactone, and rac-β-butyrolactone, and specifically may be one, two or three.

[0066] In the present invention, the lactone is preferably one or more of L-β-butyrolactone, D-β-butyrolactone, rac-β-butyrolactone, L-lactide, D-lactide, rac-lactide, meso-lactide, ε-caprolactone, γ-butyrolactone, and δ-valerolactone, and specifically can be one, two, three or four.

[0067] In the present invention, the polymerization temperature is preferably -70 to 250° C., more preferably -30 to 200° C., and most preferably 25 to 150° C. The present invention has no special requirements for the heating method of the polymerization reaction, and the heating method well known to those skilled in the art can be used.

[0068] In the present invention, the polymerization reaction is preferably carried out under an inert atmosphere. The present invention has no special requirements for the inert atmosphere, and any inert atmosphere known to those skilled in the art can be used, specifically argon.

[0069] In the present invention, the raw materials for the polymerization reaction preferably further include alcohol compounds. In the present invention, the alcohol compounds are preferably C1 to C 10 Alkyl alcohols with straight chain, branched chain or cyclic structure, or C7~C 20 The mono- or poly-aryl-substituted alkyl alcohol is more preferably C1-C 10 The most preferred linear alkyl alcohols are isopropyl alcohol and benzyl alcohol.

[0070] In the present invention, the molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the alcohol compound is 1:(0-20), more preferably 1:(0-10), and most preferably 1:(1-5).

[0071] In the present invention, the alcohol compound is used as a co-initiator to accelerate the polymerization rate and make the polymer molecular weight closer to the theoretical value and the molecular weight distribution narrower. It is used to react with the catalyst to generate a zinc alkoxy complex in situ, and further catalyze the polymerization reaction.

[0072] In the present invention, the raw materials of the polymerization reaction preferably also include a solvent, and the solvent is preferably one or more of toluene, tetrahydrofuran, and dichloromethane, and specifically can be one, two or three. The present invention has no special requirements for the order of adding the solvent, and can be mixed with the monomer and the catalyst in any order. The present invention preferably dissolves the catalyst in the solvent and configures it into a catalyst solution so that the amount of catalyst added is more controllable. In the present invention, the amount of solvent added is preferably measured in terms of the concentration of the catalyst. In the present invention, the molar concentration of the benzimidazole-substituted aminophenoloxy zinc catalyst in the solvent is preferably 0.010 to 0.030 mol / L; more preferably 0.01 to 0.028 mol / L, and most preferably 0.010 mol / L.

[0073] The present invention has no special requirements for the device used in the polymerization reaction, and any device known to those skilled in the art that can meet the technical requirements of this application can be used. In the present invention, the polymerization reaction is preferably carried out in a polymerization bottle.

[0074] In the present invention, a chain terminator is preferably added after the polymerization reaction time is reached to terminate the polymerization reaction. The present invention has no special requirements on the type of the chain terminator, and a chain terminator that can terminate the lactone polymerization reaction known to those skilled in the art can be used, and specifically, it can be a commercially available conventional solvent, such as petroleum ether, dichloromethane, n-hexane, tetrahydrofuran, methanol, etc. The present invention has no special requirements on the amount of the chain terminator, and it can be added according to the conventional technical content in this field.

[0075] After the reaction is terminated, the present invention preferably uses dichloromethane or other highly polar low boiling point solvents such as chloroform to dissolve the reactants. The present invention has no special requirements on the amount of dichloromethane used, as long as it can completely dissolve all the reactants.

[0076] After adding the dichloromethane and concentrating, the present invention preferably adds an alcohol such as methanol, ethanol, isopropanol or benzyl alcohol to precipitate the polymer product. The present invention has no special requirements on the amount of methanol added, until the precipitate no longer increases.

[0077] After the polymerization product is precipitated, the present invention preferably dries the polymerization product at 60°C to obtain the target product. The present invention has no special requirements for the specific implementation of the drying, and the drying can be carried out by a drying method of solid substances well known to those skilled in the art, specifically vacuum drying (less than 0.1 mmHg). In the present invention, the drying time is preferably 16 to 28 hours, more preferably 20 to 26 hours, and most preferably 24 hours.

[0078] The present invention provides a polymerization method of β-butyrolactone, comprising the following steps: performing a polymerization reaction on β-butyrolactone and lactone under the catalysis of a benzimidazole-substituted aminophenoloxy zinc catalyst. Compared with the prior art, the polymerization method provided by the present invention enables β-butyrolactone and lactone to be polymerized in one pot to obtain a random polymer, and the obtained polymer has a higher molecular weight.

[0079] The polymerization method of β-butyrolactone provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0080] Example 1

[0081] (1) Ligand L 4 Synthesis of H

[0082]

[0083] First, add [(1-benzyl-1H-benzimidazol-2-yl)methyl)]cyclohexylamine (10.0mmol, purity above 95%, 3.18g) and K2CO3 (15.0mmol, 2.07g) to a 250ml Schlenk bottle, replace argon gas three times under vacuum, add 50mL DMF, stir for about 10 minutes to dissolve, and the solution is dark brown. Then dissolve 2-bromomethyl-4,6-dichlorophenol (2.79g, 11.0mmol) in 40mL DMF and slowly drop it. After the dropwise addition is completed, continue to react for 12 hours. Carbon dioxide is generated during the reaction and the color of the solution becomes lighter. After the reaction is completed, extract with dichloromethane, wash with water to remove DMF, dry the organic phase with anhydrous magnesium sulfate, and remove the solvent by vacuum distillation to obtain a dark brown viscous liquid. Add 200mL methanol to dissolve the unreacted raw materials secondary amine and benzyl bromide. After stirring for one hour, change to clean methanol for washing until the solution is clear. A white solid powder (3.68 g, yield 74.6%) was obtained.

[0084] 1 H NMR(400MHz, CDCl3)δ:11.99(br s,1H,OH),7.81-7.78(m,1H,ArH),7.29-7.25(m,4H,PhH),7.24-7.22(m,2H,ArH&PhH),7.16(d, 4 J=2.5Hz,1H,ArH),6.95-6.93(m,2H,ArH),6.82-6.81(d, 4 J=2.5Hz,1H,ArH),5.38(s,2H,ArCH2),3.94(s,2H,NCH2=N),3.89(s,2H,PhCH2),2.71(m,1H,NCH of cyclohexyl),1.92-1.90(m,2H,CH2 of cyclohexyl),1.80-1.77(m,2H,CH2 of cyclohexyl),1.64-1.61(m,1H,CH2 of cyclohexyl),1.29-1.15(m,4H,CH2 of cyclohexyl),1.05(m,1H,CH2 of cyclohexyl). 13 C{ 1H}NMR (101MHz, CDCl3): δ152.45,150.85,142.07,135.72,129.16,128.55,127.67,126.07,124.94,123.23,122.71,121.61,119.98,110.41(all ArC),59.14(ArCH2),53.93(PhCH2),47.03(NCH2C=N),46.22(NCH),27.97(CH2 of cyclohexyl),26.05(CH2 of cyclohexyl),25.45(CH2 of cyclohexyl).Anal.Calcd.For C 28 H 29 Cl2N3O: C, 68.02; H, 5.91; N, 8.50. Found: C, 67.81; H, 6.01; N, 8.38%.

[0085] (2) Synthesis of Catalyst 4

[0086]

[0087] Place a 50 mL Schlenk flask and ligand L 4 H (0.439 g, 1.00 mmol) (both dried overnight in an oven at 60°C) was brought into the glove box. Zn[N(SiMe3)2]2 (0.384 g, 1.00 mmol) was weighed into a 50 mL Schlenk bottle, 5 mL of toluene was added to dissolve, and the ligand powder was added in batches. The reaction was stirred for 12 hours, and the solid gradually dissolved to form a transparent liquid. Recrystallization was performed with toluene / n-hexane to obtain a white solid powder (432 mg, yield 60.4%).

[0088] 1H NMR (400MHz, C6D6): δ7.92 (d, 3 J=8.2Hz,1H,ArH),7.15-7.12(toluene)7.06-6.97(m,8H,ArH&toluene),7.06-6.97(m,3H,ArH),6.81(t, 3 J=7.5Hz,1H,ArH),6.54-6.49(m,4H,ArH),4.46(d, 3 J=16.6Hz,1H,ArCH2),4.31(d, 3 J=16.6Hz,1H,ArCH2),3.83(d, 3 J=11.6Hz,1H,PhCH2),3.37(d, 3J=16.3Hz,1H,NCH2C=N),3.09(d, 3 J=16.3Hz,1H,NCH2C=N),2.85-2.75(m,1H,NCH),2.68(d, 3 J=11.6Hz,1H,PhCH2),2.58(br d, 3 J=10.1Hz,1H,CH2 ofcyclohexyl),2.10(s,3H,toluene),1.85(br s,1H,CH2 of cyclohexyl),1.71(br d, 3 J=12.8Hz,1H,CH2 of cyclohexyl),1.65-1.55(m,1H,CH2 of cyclohexyl),1.44(br d, 3 J=12.8Hz,1H,CH2 of cyclohexyl),1.19-0.84(m,4H,CH2 of cyclohexyl),0.55(s,18H,N(Si(CH3)3)2). 13 C{ 1 H}NMR(101MHz,C6D6):δ163.08,152.14,137.91(toluene),137.76,134.99,134.35,129.95,129.64,129.33(toluene),128.71,128.56(toluene),126.69,126.24,125.68(toluene),124.86,124.79,124.29,119.06,116.11,110.37(All ArC),76.44(NCH2C=N),55.31(NCH2Ph),49.61(ArCH2),47.01(NCH),27.54(CH2 of cyclohexyl),27.47(CH2 of cyclohexyl),26.16(CH of cyclohexyl),25.97(CH2 of cyclohexyl),25.92(CH2 of cyclohexyl),21.43(toluene),6.10(N(Si(CH3)3)2).Anal.Calcd.forC 34 H 46 Cl2N4OSi2Zn·C7H8:C,60.69;H,6.71;N,6.91.Found:C,60.31;H,6.70;N,6.80%.

[0089] Example 2

[0090] (1) Ligand L 7 Synthesis of H

[0091]

[0092] Except that the substrates were N-[(1-methyl-1H-benzimidazol-2-yl)methyl)]aniline (2.37 g, purity above 95%, 10.0 mmol), 2-(bromomethyl)-4,6-di(2-phenylpropane-2-yl)phenol (5.79 g, purity about 80%, 11.0 mmol), and K2CO3 (1.38 g, 10.0 mmol), the other experimental steps were the same as those of L 4 H. A white solid powder (4.82 g, yield 83.2%) was obtained.

[0093] 1 H NMR (400MHz, CDCl3): δ8.37(br s,1H,OH),7.66-7.64(m,1H,ArH),7.29-7.15(m,14H,ArH),6.96-6.92(m,3H,ArH),6.80(d, 4 J=2.3Hz,1H,ArH),4.43(s,2H,ArCH2),4.35(s,2H,NCH2=N),3.35(s,3H,NCH3),1.62(s,3H,CH3),1.61(s,3H,CH3). 13 C{ 1 H}NMR (101MHz, CDCl3): δ152.23,151.36,150.77,150.71,149.17,141.90,141.09,136.13,135.84,129.27,129.02,1 28.14,127.96,127.84,126.67,126.02,125.71,125.26,124.74,123.26,120.38,120.14,119.85,119.63,109.53(all ArC),54.98(PhCH2),49.95(NCH2C=N),42.58(NCH),42.18(NCH3),31.11((CH3)2CPh),31.06((CH3)2CPh),29.77((CH3)2CPh).Anal.Calcd.For C 40 H 41 N3O: C, 82.86; H, 7.13; N, 7.25. Found: C, 82.74; H, 7.12; N, 7.30%.

[0094] (2) Synthesis of Catalyst 7

[0095]

[0096] Except for the reactant L 7 Except for H (0.579 g, 1.00 mmol) and Zn[N(SiMe3)2]2 (0.384 g, 1.00 mmol), other experimental steps were the same as Zn4. Recrystallization gave a white solid powder (421 mg, yield 52.5%).

[0097] 1 H NMR (400MHz, C6D6): δ7.72-7.70(d, 3 J=8.3Hz,1H,ArH),7.25-6.86(m,18H,ArH),6.56(d, 3 J=7.9Hz,1H,ArH),6.45(d, 3 J=2.5Hz,1H,ArH),4.52(d, 3 J=11.4Hz,1H,ArCH2),3.51(s,2H,ArCH2),2.93(d, 3 J=11.0Hz,1H,ArCH2),2.18(s,3H,NCH3),1.74(s,3H,CH3),1.56(s,3H,CH3),1.50(s,3H,CH3),1.44(s,3H,CH3),0.29(s,18H,N(Si(CH3)3)2). 13 C{ 1 H}NMR (101MHz, C6D6): δ164.87,152.68,152.31,151.34,138.53,137.77,135.17,133.16,129.51,128.23,128.1 8,127.94,127.74,126.97,126.74,125.83,125.44,124.82,123.97,123.93,122.58,121.46,119.56,109.54(All ArC),65.79(ArCH2),51.18(NCH2C=N),43.31(PhC(CH3)2),42.20(PhC(CH3)2),31.88,31. 32,31.02,28.54(PhC(CH3)2),28.28(NCH3),26.78,6.08(N(Si(CH3)3)2).Anal.Calcd.for C 46 H 58N4OSi2Zn:C,68.67;H,7.27;N,6.96.Found:C,68.37;H,7.23;N,7.03.

[0098] Example 3

[0099] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[Cat.]:[ i PrOH]=200:1:1. The reaction temperature was controlled at 25°C, the reaction was carried out for 1.5h, and petroleum ether was added to terminate the reaction.

[0100] Dissolve it in dichloromethane and take a sample to measure the H NMR spectrum. The calculation shows that the conversion rate of rac-β-butyrolactone is 87%, TOF = 116h -1 ; Polymer syntacticity: 0.64.

[0101] After the remaining solution was concentrated, methanol was added to precipitate the polymer and dried in vacuum for 24 hours. Samples were taken for GPC analysis and M n =1.6×10 4 g / mol, molecular weight distribution PDI=1.32.

[0102] Example 4

[0103] Except that the solvent was changed to tetrahydrofuran and the reaction time was 4.0 hours, the other conditions were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 89% and TOF was 44 hours. -1 ; Polymer syntacticity: 0.62. M n =1.4×10 4 g / mol, molecular weight distribution PDI=1.33.

[0104] Example 5

[0105] Except that the catalyst was replaced with 3 and the reaction was continued for 1.5 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 82% and TOF was 109h. -1 ; Polymer syntacticity: 0.58; M n =1.5×10 4 g / mol, molecular weight distribution PDI=1.38.

[0106] Example 6

[0107] Except that the solvent was replaced by tetrahydrofuran, the catalyst was replaced by 2, and the reaction was continued for 5.5 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 82% and TOF was 30 hours.-1 ; Polymer syntacticity: 0.63; M n =1.2×10 4 g / mol, molecular weight distribution PDI=1.32.

[0108] Example 7

[0109] Except that the catalyst was replaced with 3 and the reaction time was 7.7 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 90% and TOF was 23 hours. -1 ; Polymer syntacticity: 0.60; M n =1.4×10 4 g / mol, molecular weight distribution PDI=1.32.

[0110] Example 8

[0111] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of toluene solution of catalyst 3 and add it into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[Cat.]:[ i PrOH]=200:1:0. Control the reaction temperature at 25℃, react for 35.0h, and add petroleum ether to terminate the reaction. The conversion rate of rac-β-butyrolactone is 98% and TOF=6h -1 ; Polymer syntacticity: 0.61. M n =1.8×10 4 g / mol, molecular weight distribution PDI=1.39.

[0112] Example 9

[0113] Except that the solvent was replaced by tetrahydrofuran, the catalyst was replaced by 3, and the reaction was continued for 11.5 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 79% and TOF was 14 hours. -1 ; Polymer syntacticity: 0.59; M n =1.6×10 4 g / mol, molecular weight distribution PDI=1.19.

[0114] Example 10

[0115] Except that the catalyst was replaced with 4 and the reaction time was 4.0 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 95% and TOF was 47 hours. -1 ; Polymer syntacticity: 0.60; M n =1.2×10 4 g / mol, molecular weight distribution PDI=1.23.

[0116] Embodiment 11

[0117] Except that the solvent was replaced by tetrahydrofuran, the catalyst was replaced by 4, and the reaction was carried out for 8.0 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 81% and TOF was 20 hours. -1 ; Polymer syntacticity: 0.64; M n =1.8×10 4 g / mol, molecular weight distribution PDI=1.23.

[0118] Example 12

[0119] Except that the catalyst was replaced with 5 and the reaction time was 8.0 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 91% and TOF was 23h. -1 ; Polymer syntacticity: 0.59; M n =1.2×10 4 g / mol, molecular weight distribution PDI=1.33.

[0120] Example 13

[0121] Except that the solvent was replaced by tetrahydrofuran, the catalyst was replaced by 5, and the reaction was continued for 13.0 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 81% and TOF was 12 hours. -1 ; Polymer syntacticity: 0.59; M n =1.5×10 4 g / mol, molecular weight distribution PDI=1.15.

[0122] Embodiment 14

[0123] Except that the catalyst was replaced with 6 and the reaction was continued for 1.5 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 93% and TOF was 46 hours. -1 ; Polymer syntacticity: 0.59; M n =1.3×10 4 g / mol, molecular weight distribution PDI=1.38.

[0124] Embodiment 15

[0125] Except that the solvent was replaced by tetrahydrofuran, the catalyst was replaced by 6, and the reaction time was 7.0 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 80%, and TOF was 23 hours. -1 ; Polymer syntacticity: 0.62; M n =1.2×10 4 g / mol, molecular weight distribution PDI=1.24.

[0126] Example 16

[0127] Except that the catalyst was replaced with 7 and the reaction was continued for 1.5 h, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 84% ​​and TOF was 112 h. -1 ; Polymer syntacticity: 0.58; M n =1.8×10 4 g / mol, molecular weight distribution PDI=1.68.

[0128] Embodiment 17

[0129] Except that the solvent was replaced by tetrahydrofuran, the catalyst was replaced by 7, and the reaction time was 9.0 hours, the other operations were the same as in Example 3. The conversion rate of rac-β-butyrolactone was 92% and TOF was 20 hours. -1 ; Polymer syntacticity: 0.56; M n =1.5×10 4 g / mol, molecular weight distribution PDI=1.23.

[0130] Embodiment 18

[0131] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol), rac-lactide (288 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[LA]:[Cat.]:[ i PrOH]=200:200:1:1. The reaction temperature was controlled at 25℃, the reaction lasted for 270min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 25%, and the conversion rate of rac-lactide was >99%. M n =3.1×10 4 g / mol, molecular weight distribution PDI=1.46.

[0132] Embodiment 19

[0133] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol), rac-lactide (288 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[LA]:[Cat.]:[ iPrOH]=200:200:1:1. The reaction temperature was controlled at 25℃, and the reaction was continued for 24h. Petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 66% and the conversion rate of rac-lactide was >99%. n =2.6×10 4 g / mol, molecular weight distribution PDI=1.57.

[0134] Embodiment 20

[0135] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol), L-lactide (288 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[LA]:[Cat.]:[ i PrOH]=200:200:1:1. The reaction temperature was controlled at 25℃, the reaction was continued for 18h, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 70%, and the conversion rate of L-lactide was >99%. n =1.05×10 5 g / mol, molecular weight distribution PDI=1.53.

[0136] Embodiment 21

[0137] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol), ε-caprolactone (228 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[CL]:[Cat.]:[ i PrOH]=200:200:1:1. Control the reaction temperature at 25℃, react for 10min, and add petroleum ether to terminate the reaction. According to the test and calculation, the conversion rate of rac-β-butyrolactone is 45%, and the conversion rate of ε-caprolactone is 52%. M n =4.6×10 4 g / mol, molecular weight distribution PDI=1.52.

[0138] Embodiment 22

[0139] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol), ε-caprolactone (228 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[CL]:[Cat.]:[i PrOH]=200:200:1:1. The reaction temperature was controlled at 25℃, the reaction was continued for 60min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 74% and the conversion rate of ε-caprolactone was 85%. n =3.9×10 4 g / mol, molecular weight distribution PDI=1.50.

[0140] Embodiment 23

[0141] Under argon protection, add rac-β-butyrolactone (69 mg, 2 mmol), ε-caprolactone (365 mg, 3.2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[CL]:[Cat.]:[ i PrOH]=80:320:1:1. The reaction temperature was controlled at 25℃, the reaction was continued for 60min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 99% and the conversion rate of ε-caprolactone was 99%. M n =4.7×10 4 g / mol, molecular weight distribution PDI=1.60.

[0142] Embodiment 24

[0143] Under argon protection, add rac-β-butyrolactone (275 mg, 3.2 mmol), ε-caprolactone (91 mg, 0.8 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [β-BL]:[CL]:[Cat.]:[ i PrOH]=320:80:1:1. The reaction temperature was controlled at 25℃, the reaction was continued for 60min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 55% and the conversion rate of ε-caprolactone was 63%. M n =2.0×10 4 g / mol, molecular weight distribution PDI=1.34.

[0144] Embodiment 25

[0145] Under argon protection, add rac-β-butyrolactone (172 mg, 2 mmol), ε-caprolactone (228 mg, 2 mmol) and 0.9 mL toluene into the polymerization bottle. Measure 0.1 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.002M, [β-BL]:[CL]:[Cat.]:[ i PrOH]=1000:1000:1:1. The reaction temperature was controlled at 25℃, the reaction lasted for 150min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 80% and the conversion rate of ε-caprolactone was 89%. n =2.0×10 5 g / mol, molecular weight distribution PDI=1.55.

[0146] Embodiment 26

[0147] Under argon protection, add rac-β-butyrolactone (275 mg, 3.2 mmol), ε-caprolactone (91 mg, 0.8 mmol) and 0.9 mL toluene into the polymerization bottle. Measure 0.1 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.002M, [β-BL]:[CL]:[Cat.]:[ i PrOH]=1600:400:1:1. The reaction temperature was controlled at 25℃, the reaction lasted for 170min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 45% and the conversion rate of ε-caprolactone was 58%. M n =1.1×10 5 g / mol, molecular weight distribution PDI=1.45.

[0148] Embodiment 27

[0149] Under argon protection, add rac-β-butyrolactone (69 mg, 2 mmol), ε-caprolactone (365 mg, 3.2 mmol) and 0.9 mL toluene into the polymerization bottle. Measure 0.1 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.002M, [β-BL]:[CL]:[Cat.]:[ i PrOH]=400:1600:1:1. The reaction temperature was controlled at 25℃, the reaction lasted for 110min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-β-butyrolactone was 89% and the conversion rate of ε-caprolactone was 95%. n =1.9×10 5 g / mol, molecular weight distribution PDI=1.52.

[0150] Embodiment 28

[0151] Under argon protection, add rac-lactide (288 mg, 2 mmol), ε-caprolactone (228 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [LA]:[CL]:[Cat.]:[ i PrOH]=200:200:1:1. The reaction temperature was controlled at 25℃, and the reaction was continued for 23h. Petroleum ether was added to terminate the reaction. The conversion rate of rac-lactide was calculated to be >99%, and the conversion rate of ε-caprolactone was 86%. n =3.8×10 4 g / mol, molecular weight distribution PDI=1.46.

[0152] Embodiment 29

[0153] Under argon protection, add rac-lactide (288 mg, 2 mmol), ε-caprolactone (228 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [LA]:[CL]:[Cat.]:[ i PrOH]=200:200:1:1. The reaction temperature was controlled at 25℃, and the reaction was continued for 25h. Petroleum ether was added to terminate the reaction. The conversion rate of rac-lactide was calculated to be >99%, and the conversion rate of ε-caprolactone was 92%. n =3.1×10 4 g / mol, molecular weight distribution PDI=1.48.

[0154] Embodiment 30

[0155] Under argon protection, add rac-β-butyrolactone (86 mg, 1 mmol), L-lactide (144 mg, 1 mmol), ε-caprolactone (114 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [LA]:[CL]:[β-BL]:[Cat.]:[ i PrOH]=100:100:100:1:1. The reaction temperature was controlled at 25℃, the reaction lasted for 180min, and petroleum ether was added to terminate the reaction. The results of the test and calculation showed that the conversion rate of L-lactide was >99%, the conversion rate of rac-β-butyrolactone was 26%, and the conversion rate of ε-caprolactone was 28%. n =1.9×10 4 g / mol, molecular weight distribution PDI=1.64.

[0156] Embodiment 31

[0157] Under argon protection, add rac-β-butyrolactone (86 mg, 1 mmol), L-lactide (144 mg, 1 mmol), ε-caprolactone (114 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [LA]:[CL]:[β-BL]:[Cat.]:[ i PrOH]=100:100:100:1:1. The reaction temperature was controlled at 25℃, the reaction lasted for 480min, and petroleum ether was added to terminate the reaction. The results of the test and calculation showed that the conversion rate of L-lactide was >99%, the conversion rate of rac-β-butyrolactone was 51%, and the conversion rate of ε-caprolactone was 60%. n =1.1×10 4 g / mol, molecular weight distribution PDI=1.73.

[0158] Embodiment 32

[0159] Under argon protection, add rac-β-butyrolactone (86 mg, 1 mmol), rac-lactide (144 mg, 1 mmol), ε-caprolactone (114 mg, 2 mmol) and 0.5 mL toluene into the polymerization bottle. Measure 0.5 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [LA]:[CL]:[β-BL]:[Cat.]:[ i PrOH]=100:100:100:1:1. The reaction temperature was controlled at 25℃, the reaction lasted for 350min, and petroleum ether was added to terminate the reaction. The conversion rate of rac-lactide was>99%, the conversion rate of rac-β-butyrolactone was 52%, and the conversion rate of ε-caprolactone was 58%. M n =1.8×10 4 g / mol, molecular weight distribution PDI=1.66.

[0160] Embodiment 33

[0161] Under argon protection, add rac-β-butyrolactone (86 mg, 1 mmol), rac-lactide (144 mg, 1 mmol), ε-caprolactone (114 mg, 2 mmol) and 0.9 mL toluene into the polymerization bottle. Measure 0.1 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [LA]:[CL]:[β-BL]:[Cat.]:[ iPrOH]=500:500:500:1:1. The reaction temperature was controlled at 25℃, the reaction was continued for 11h, and petroleum ether was added to terminate the reaction. The conversion rate of rac-lactide was>99%, the conversion rate of rac-β-butyrolactone was 70%, and the conversion rate of ε-caprolactone was 78%. M n =2.8×10 5 g / mol, molecular weight distribution PDI=1.66.

[0162] Embodiment 34

[0163] Under argon protection, add rac-β-butyrolactone (86 mg, 1 mmol), rac-lactide (144 mg, 1 mmol), ε-caprolactone (114 mg, 2 mmol) and 0.9 mL toluene into the polymerization bottle. Measure 0.1 mL of catalyst 1 and isopropanol toluene solution and add them into the polymerization bottle. Make [Cat.]0=0.01M, [LA]:[CL]:[β-BL]:[Cat.]:[ i PrOH]=500:500:500:1:1. Control the reaction temperature to 110℃, react for 3h, and add petroleum ether to terminate the reaction. According to the test and calculation, the conversion rate of rac-lactide:>99%, the conversion rate of rac-β-butyrolactone:68%, and the conversion rate of ε-caprolactone:78%. M n =1.9×10 5 g / mol, molecular weight distribution PDI=1.76.

[0164] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A polymerization method for β-butyrolactone, comprising the following steps: The β-butyrolactone and lactone are polymerized under the catalytic condition of benzimidazole-substituted aminophenoloxy zinc catalyst; The benzimidazole-substituted aminophenoloxy zinc catalyst has a structure shown in formula (I): In the formula (I): R 1 ~R 2 Represent hydrogen, C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 mono- or poly-aryl-substituted alkyl, halogen; R 3 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 Mono- or poly-aryl-substituted alkyl, C6~C 18 The aromatic group; R 4 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 A mono- or poly-aryl-substituted alkyl group; X represents amino group NR 5 R 6 , where R 5 ~R 6 are C1-C6 straight chain, branched chain or cyclic alkyl, trimethylsilyl, triethylsilyl, dimethylhydrogensilyl, R 5 and R 6 Can be the same or different.

2. The polymerization method according to claim 1, characterized in that In the formula (I), R 1 ~R 2 are hydrogen, C1-C8 straight chain, branched chain or cyclic alkyl, C7-C 20 mono- or poly-aryl-substituted alkyl, halogen; R 3 It is a C1-C8 straight chain, branched chain or cyclic alkyl group, C7-C 20 Mono- or poly-aryl-substituted alkyl, C6~C 12 The aryl group; R 4 It is a C1-C8 straight chain, branched chain or cyclic alkyl group, C7-C 20 The mono- or poly-aryl-substituted alkyl group; X is bis(trimethylsilyl)amino, bis(triethylsilyl)amino, bis(dimethylhydrogensilyl)amino.

3. The polymerization method according to claim 1, characterized in that In the formula (I), R 1 ~R 2 are methyl, tert-butyl, cumyl, trityl, and chlorine respectively; R 3 is methyl, ethyl, isopropyl, n-butyl, tert-butyl, isopentyl, cyclohexyl, cyclopentyl, n-hexyl, n-octyl, benzyl, phenethyl, or phenyl; R 4 is methyl, ethyl, isopropyl, n-butyl, cyclohexyl, cyclopentyl, benzyl, phenethyl; X is bis(trimethylsilyl)amino.

4. The polymerization method according to claim 1, characterized in that: The molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to β-butyrolactone is 1:(50-10000); The molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the lactone is 1:(0-10000).

5. The polymerization method according to claim 1, characterized in that: The molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to β-butyrolactone is 1:(50-5000); The molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the lactone is 1:(0-5000).

6. The polymerization method according to claim 1, characterized in that The β-butyrolactone is one or more of L-β-butyrolactone, D-β-butyrolactone and rac-β-butyrolactone.

7. The polymerization method according to claim 1, characterized in that The lactone is one or more of L-β-butyrolactone, D-β-butyrolactone, rac-β-butyrolactone, L-lactide, D-lactide, rac-lactide, meso-lactide, ε-caprolactone, γ-butyrolactone and δ-valerolactone.

8. The polymerization method according to claim 1, characterized in that The polymerization reaction temperature is -70 to 250° C.; the polymerization reaction is carried out under an inert atmosphere.

9. The polymerization method according to any one of claims 1 to 8, characterized in that The raw materials for the polymerization reaction also include alcohol compounds; the molar ratio of the benzimidazole-substituted aminophenoloxy zinc catalyst to the alcohol compound is 1:(0-20).

10. The polymerization method according to claim 8, characterized in that The alcohol compound is C1~C 10 Alkyl alcohols with straight chain, branched chain or cyclic structure, or C7~C 20 Mono- or poly-aryl-substituted alkyl alcohols.

Citation Information

Patent Citations

  • Imidazole ring substituted aminophenol oxy-zinc complex and preparation method and application thereof

    CN109879810A

  • Aminophenol oxygroup zinc complex containing chiral tetrahydropyrrole skeleton as well as preparation method and application of aminophenol oxygroup zinc complex

    CN114349781A

  • Benzimidazole substituted aminophenol oxygroup zinc halide as well as preparation method and application thereof

    CN114507246A

  • Polymerization method of substituted glycolide

    CN116948155A

  • Epoxy compound, anhydride and lactone copolymerization method

    CN118406219A