Anti-puncture inner tube material and preparation method thereof

By modifying materials such as natural rubber, modified aramid fiber and end aminopolysiloxane, an anti-puncture inner tube material is formed, which solves the problems of easy damage and insufficient durability of the inner tube material, and achieves good anti-puncture, Flame retardant and wear resistance improve the overall performance of the tire.

CN119060421AInactive Publication Date: 2024-12-03NANTONG SUNCHI RUBBER PROD CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411558381.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing inner tube materials are prone to damage when facing external forces such as pulling, pulling, and pricking, and are insufficient in durability and flame retardant performance, making it difficult to meet the high requirements of tires.

Method used

The reaction is carried out using natural rubber, modified aramid fiber and end aminopolysiloxane and other materials, and then modified with a mixed solution of N-(trifluoromethylthio)phthalimide to form a puncture-proof inner tube material. The enhancement of the material's puncture, flame retardant and wear resistance is achieved through the combination of electrospinning of aramid fibers and self-healing gels.

Benefits of technology

It significantly improves the puncture resistance of the inner tube, extends the service life, enhances the flame retardant and wear resistance, and improves the overall durability and safety of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an anti-puncture inner tube material and a preparation method thereof, and relates to the field of high polymer materials. When the anti-puncture inner tube material is prepared, 3-aminopropyl methyl dimethoxy silane firstly reacts with salicylaldehyde and then reacts with 1, 3-bis (3-aminopropyl) tetramethyldisiloxane and dimethoxy dimethyl silane, and amino-terminated polysiloxane is prepared; the preparation method comprises the following steps: reacting poloxamer, triethylamine, acryloyl chloride and dichloromethane, and polymerizing a polyester monomer to prepare self-repairing gel; reacting the diamine mixture with terephthaloyl chloride to prepare an aramid fiber emulsion; carrying out coaxial electrostatic spinning on the aramid emulsion and the self-repairing gel, and then reacting with the modified nano silicon dioxide to prepare modified aramid fibers; the preparation method comprises the following steps: reacting natural rubber, modified aramid fiber and amino-terminated polysiloxane, and modifying with an N-(trifluoromethylthio) phthalimide mixed solution to obtain the anti-puncture inner tube material. The anti-puncture inner tube material prepared by the invention has wear-resistant, anti-aging, flame-retardant and anti-puncture effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer materials, in particular to a puncture-proof inner tube material and a preparation method thereof. Background Art

[0002] Tires are one of the main components of automobiles, tractors and engineering vehicles. Their function is to support the weight of the vehicle, transmit traction, steering force and braking force, and absorb the vibration caused by uneven roads. Generally speaking, tires are composed of three parts: outer tube, inner tube and cushion belt. The inner tube is an annular rubber cylinder installed between the outer tube and the wheel. After being filled with air, the tire can gain elasticity and load-bearing capacity.

[0003] The inner tube is a ring-shaped rubber tube with a valve nozzle, which is used to maintain the inflation pressure of the tire. It is also the main bearer of the car load. Therefore, the inner tube is often in conditions of extension and flexion deformation and large temperature changes. It is also often pulled, stretched and punctured, and is easily damaged. Therefore, this article introduces an anti-puncture inner tube material with aging resistance. Summary of the invention

[0004] The purpose of the present invention is to provide a puncture-resistant inner tube material and a preparation method thereof, so as to solve the problems existing in the prior art.

[0005] A puncture-proof inner tube material, which is prepared by reacting natural rubber, modified aramid fiber, and amino-terminated polysiloxane and then modifying with a mixed solution of N-(trifluoromethylthio)phthalimide; The amino-terminated polysiloxane is prepared by first reacting 3-aminopropylmethyldimethoxysilane with salicylaldehyde and then reacting with 1,3-bis(3-aminopropyl)tetramethyldisiloxane and dimethoxydimethylsilane; The modified aramid fiber is prepared by coaxially electrospinning aramid emulsion and self-repairing gel, and then reacting with modified nano-silicon dioxide; The aramid emulsion is prepared by reacting a diamine mixture with terephthaloyl chloride; The self-repairing gel is prepared by reacting poloxamer, triethylamine, acryloyl chloride and dichloromethane and then polymerizing polyester monomers therein.

[0006] A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) 3-aminopropylmethyldimethoxysilane, salicylaldehyde and ethanol were mixed in a mass ratio of 1:1:10-12, reacted at 24-26°C and 25-35 r / min for 5-7 h, and vacuum dried at 55-65°C for 4-6 h to obtain anti-aging siloxane; 1,3-bis(3-aminopropyl)tetramethyldisiloxane, anti-aging siloxane, dimethoxydimethylsilane, deionized water and 36-38% hydrochloric acid solution were mixed in a mass ratio of 1:1:10-12, reacted at 24-26°C and 25-35 r / min for 5-7 h, and vacuum dried at 55-65°C for 4-6 h to obtain anti-aging siloxane; Mix in a mass ratio of 14-16:50-70:100-110:300-500:1-3, stir at 200-300 r / min for 25-35 min, heat to 50-60°C, continue stirring for 2.5-3.5 h, add sodium carbonate in an amount of 0.03-0.05 times the mass of dimethoxydimethylsilane, continue stirring for 20-30 min, dry at 80-100°C for 20-24 h to obtain amino-terminated polysiloxane; (2) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:10-11:10-11:26-28, stirred at 200-300 r / min for 23-25 ​​h, filtered to obtain the filtrate, dried the filtrate at 36-38 °C for 1-2 h, immersed in methyl tert-butyl ether, allowed to stand for 10-20 min, filtered, and vacuum dried for 23-25 ​​h to obtain polyether F127 dipropylene Acid ester; at -4~0°C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine are mixed in a molar ratio of 0.005~0.007:1100~1200:95~105:0.4~0.45:0.7~0.8, stirred at 200~300r / min for 15~25min, heated to room temperature, and allowed to stand under vacuum for 22~26h to obtain a self-healing gel; (3) Mix methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine in a molar ratio of 1:1, add a catalyst in an amount of 0.03 to 0.05 times the mass of methyldimethoxysilane, and react at 60 to 70°C for 4 to 6 hours to obtain modified siloxane; (4) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed uniformly in a mass ratio of 1:51~52, stirred at 70~90℃ and 200~300r / min for 20~30min, cooled to room temperature, added with diamine mixture, continued stirring for 10~20min, added terephthaloyl chloride with 0.45~0.5 times the molar weight of the amino group in the diamine mixture and pyridine with 0.04~0.06 times the volume of N-methylpyrrolidone, stirred at -6~-4℃ and 1100~1300r / min for 15~25min, and heated to room temperature. temperature, and continue stirring for 25-35 minutes to obtain aramid emulsion; use aramid emulsion as shell solution and self-healing gel as core solution to carry out coaxial electrospinning, stand for 6-8 hours, and naturally cool to room temperature to obtain pre-modified aramid fiber; modify nano-silica, modified aramid fiber and isopropanol are mixed uniformly in a mass ratio of 1:6-8:16-18, stir at 85-95°C and 200-300r / min for 5-7 hours, centrifuge to obtain solid, wash with deionized water for 3-5 times, and dry at 90-100°C for 2-4 hours to obtain modified aramid fiber; (5) Under argon protection, natural rubber, modified aramid fiber, amino-terminated polysiloxane and ethanol are mixed in a mass ratio of 9-11:3-5:1-2:20-30, stirred at 45-55°C and 300-400 r / min for 3-5 h, vacuum dried at 60-70°C for 11-13 h, and vulcanized to obtain a modified rubber; the modified rubber is immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 48-50 h, taken out, immersed in deionized water for ultrasonic treatment for 10-20 min, and dried at -10--1°C under vacuum conditions for 22-24 h to obtain a puncture-resistant inner tube.

[0007] As an optimization, the polyester monomer in step (2) is prepared by uniformly mixing methyl methacrylate, 4-vinylbenzene boronic acid and 3-butene-1,2-diol in a molar ratio of 4-6:1:1.

[0008] As an optimization, the catalyst in step (3) is prepared by uniformly mixing chloroplatinic acid and isopropanol in a mass ratio of 1:75-82.

[0009] As an optimization, the modified nano-silica in step (4) is prepared by uniformly mixing nano-silica, 3-aminopropyltrimethoxysilane and isopropanol in a mass ratio of 1:1:6-8, stirring the mixture at 85-95°C and 200-300 r / min for 5-7 hours, centrifuging the solid, washing it with deionized water for 3-5 times, and drying it at 90-100°C for 2-4 hours.

[0010] As an optimization, the diamine mixture in step (4) is prepared by uniformly mixing meta-phenylenediamine, para-phenylenediamine and modified siloxane in a molar ratio of 0.5-0.6:1:0.1-0.2.

[0011] As an optimization, the liquid flow rate of the shell solution in step (4) is 0.9-1.1 ml / h.

[0012] As an optimization, the liquid flow rate of the core solution in step (4) is 0.2-0.3 ml / h.

[0013] As an optimization, the vulcanization in step (5) is carried out on a flat vulcanizing press with the following parameters: the size of the upper and lower heating plates is 30 cm × 30 cm, the temperature range of the upper platen of the press is 0-300°C, the temperature range of the lower platen is 0-300°C, and the pressure range of the press is 0-40 MPa.

[0014] As an optimization, the N-(trifluoromethylthio)phthalimide mixed solution in step (5) is prepared by uniformly mixing N-(trifluoromethylthio)phthalimide, acetonitrile and benzophenone in a mass ratio of 7-8:0.5-1:49-53.

[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: When preparing the puncture-proof inner tube material, the present invention first reacts 3-aminopropylmethyldimethoxysilane with salicylaldehyde and then reacts with 1,3-bis(3-aminopropyl)tetramethyldisiloxane and dimethoxydimethylsilane to obtain amino-terminated polysiloxane; poloxamer, triethylamine, acryloyl chloride and dichloromethane are reacted and then polyester monomer is polymerized therein to obtain self-repairing gel; a diamine mixture is reacted with terephthaloyl chloride to obtain aramid emulsion; the aramid emulsion and the self-repairing gel are coaxially electrospun and then reacted with modified nano-silica to obtain modified aramid fiber; natural rubber, modified aramid fiber and amino-terminated polysiloxane are reacted and then modified with a mixed solution of N-(trifluoromethylthio)phthalimide to obtain the puncture-proof inner tube material.

[0016] First, 3-aminopropylmethyldimethoxysilane is reacted with salicylaldehyde and then with 1,3-bis(3-aminopropyl)tetramethyldisiloxane and dimethoxydimethylsilane to obtain amino-terminated polysiloxane; 3-aminopropylmethyldimethoxysilane is first reacted with salicylaldehyde to generate an anti-aging structure, which prolongs the service life of the inner tube, and when the silicon-oxygen chain burns, the silicon-oxygen bond in the molecule will be converted into a silicon-carbon bond, forming a composite carbon layer together with the generated carbonized product. This composite carbon layer has the advantages of blocking heat, isolating oxygen, and preventing molten droplets, which seals the polymer material, prevents the flammable gas from diffusing outward, and improves the flame retardant ability of the material. The use of amino end-capping can react with the double bond on the natural rubber in the subsequent reaction to enhance the bonding effect.

[0017] Secondly, poloxamer, triethylamine, acryloyl chloride and dichloromethane are reacted, and then the polyester monomer is polymerized therein to obtain a self-repairing gel; the diamine mixture is reacted with terephthaloyl chloride to obtain an aramid emulsion; the aramid emulsion and the self-repairing gel are coaxially electrospun, and then reacted with modified nano-silica to obtain modified aramid fibers; natural rubber, modified aramid fibers, and terminal amino polysiloxane are reacted and then modified with a mixed solution of N-(trifluoromethylthio)phthalimide to obtain a puncture-resistant inner tube material. The coaxial electrospinning of the aramid emulsion and the self-repairing gel can produce a material with excellent effect. The puncture-proof material can enhance the puncture-proof ability of the inner tube. The aramid fiber can decompose to produce non-flammable gas after absorbing heat. On the one hand, it can dilute the concentration of oxygen in the air and combustibles produced by the thermal decomposition of the polymer. On the other hand, the nitrogen oxides produced by the decomposition can capture free radicals, making the material flame retardant. Silica can enhance the wear resistance of the inner tube, and the surface of silica is rich in amino groups, which can have a better bonding effect with natural rubber. With fluorine modification, the surface tension of fluorine-containing polymers is extremely low and the stability is very high, which can further enhance the durability of the inner tube.‌ DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1

[0019] A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) 3-aminopropylmethyldimethoxysilane, salicylaldehyde and ethanol were mixed in a mass ratio of 1:1:10, reacted at 24°C and 25 r / min for 5 h, and vacuum dried at 55°C for 4 h to obtain anti-aging siloxane; 1,3-bis(3-aminopropyl)tetramethyldisiloxane, anti-aging siloxane, dimethoxydimethylsilane, deionized water and 36% hydrochloric acid solution were mixed in a mass ratio of 14:50:100:300:1, stirred at 200 r / min for 25 min, heated to 50°C, continued to stir for 2.5 h, added sodium carbonate 0.03 times the mass of dimethoxydimethylsilane, continued to stir for 20 min, and dried at 80°C for 20 h to obtain terminal amino polysiloxane; (2) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:10:10:26, stirred at 200 r / min for 23 h, filtered and the filtrate was dried at 36 ° C for 1 h, immersed in methyl tert-butyl ether, allowed to stand for 10 min, filtered, and vacuum dried for 23 h to obtain polyether F127 diacrylate; at -4 ° C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine were mixed in a molar ratio of 0.005:1100:95:0.4:0.7, stirred at 200 r / min for 15 min, heated to room temperature, and allowed to stand under vacuum for 22 h to obtain a self-healing gel; (3) Methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine were mixed in a molar ratio of 1:1, a catalyst in an amount of 0.03 times the mass of methyldimethoxysilane was added, and the mixture was reacted at 60°C for 4 hours to obtain modified siloxane; (4) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:51, stirred at 70°C and 200 r / min for 20 min, cooled to room temperature, added with the diamine mixture, and continued to stir for 10 min. Then, 0.45 times the molar amount of terephthaloyl chloride of the diamine mixture and 0.04 times the volume of pyridine of N-methylpyrrolidone were added, stirred at -6°C and 1100 r / min for 15 min, heated to room temperature, and continued to stir. Stir for 25 minutes to obtain aramid emulsion; use aramid emulsion as shell solution and self-healing gel as core solution to carry out coaxial electrospinning, let stand for 6 hours, and naturally cool to room temperature to obtain pre-modified aramid fiber; modify nano-silica, modify aramid fiber and isopropanol are mixed evenly in a mass ratio of 1:6:16, stirred at 85°C and 200r / min for 5 hours, centrifuged to obtain solid, washed with deionized water 3 times, and dried at 90°C for 2 hours to obtain modified aramid fiber; (5) Under argon protection, natural rubber, modified aramid fiber, terminal amino polysiloxane and ethanol were mixed in a mass ratio of 9:3:1:20, stirred at 45°C and 300 r / min for 3 h, vacuum dried at 60°C for 11 h, and vulcanized to obtain a modified rubber; the modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 48 h, taken out, immersed in deionized water for 10 min, and dried at -10°C under vacuum conditions for 22 h to obtain a puncture-resistant inner tube. Example 2

[0020] A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) 3-aminopropylmethyldimethoxysilane, salicylaldehyde and ethanol were mixed in a mass ratio of 1:1:11, reacted at 25°C and 30 r / min for 6 h, and vacuum dried at 60°C for 5 h to obtain anti-aging siloxane; 1,3-bis(3-aminopropyl)tetramethyldisiloxane, anti-aging siloxane, dimethoxydimethylsilane, deionized water and 37% hydrochloric acid solution were mixed in a mass ratio of 15:60:105:400:2, stirred at 250 r / min for 30 min, heated to 55°C, and continued to stir for 3 h, added sodium carbonate 0.04 times the mass of dimethoxydimethylsilane, continued to stir for 25 min, and dried at 90°C for 22 h to obtain terminal amino polysiloxane; (2) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:10.5:10.5:27, stirred at 250 r / min for 24 h, filtered and the filtrate was dried at 37 ° C for 1.5 h, immersed in methyl tert-butyl ether, allowed to stand for 15 min, filtered, and vacuum dried for 24 h to obtain polyether F127 diacrylate; at -2 ° C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine were mixed in a molar ratio of 0.006:1150:100:0.425:0.75, stirred at 250 r / min for 20 min, heated to room temperature, and allowed to stand under vacuum for 24 h to obtain a self-healing gel; (3) Methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine were mixed in a molar ratio of 1:1, a catalyst in an amount of 0.04 times the mass of methyldimethoxysilane was added, and the mixture was reacted at 65°C for 5 hours to obtain modified siloxane; (4) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:51.5, stirred at 80°C and 250 r / min for 25 min, cooled to room temperature, added with the diamine mixture, and stirred for 15 min. Then, 0.475 times the molar amount of terephthaloyl chloride of the diamine mixture and 0.05 times the volume of pyridine of N-methylpyrrolidone were added, stirred at -5°C and 1200 r / min for 20 min, heated to room temperature, and then stirred for 15 min. The mixture was stirred for 30 min to obtain an aramid emulsion; the aramid emulsion was used as the shell solution and the self-healing gel was used as the core solution for coaxial electrospinning, and the mixture was allowed to stand for 7 h and naturally cooled to room temperature to obtain a pre-modified aramid fiber; the modified nano-silica, the modified aramid fiber and isopropanol were uniformly mixed in a mass ratio of 1:7:17, stirred at 90°C and 250 r / min for 6 h, the solid was separated by centrifugation, washed with deionized water 4 times, and dried at 95°C for 3 h to obtain the modified aramid fiber; (5) Under argon protection, natural rubber, modified aramid fiber, amino-terminated polysiloxane and ethanol were mixed in a mass ratio of 10:4:1.5:25, stirred at 50°C and 350 r / min for 4 h, vacuum dried at 65°C for 12 h, and vulcanized to obtain a modified rubber; the modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 49 h, taken out, immersed in deionized water for 15 min, and dried at -5.5°C under vacuum conditions for 23 h to obtain a puncture-resistant inner tube. Example 3

[0021] A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) 3-aminopropylmethyldimethoxysilane, salicylaldehyde and ethanol were mixed in a mass ratio of 1:1:12, reacted at 26°C and 35 r / min for 7 hours, and vacuum dried at 65°C for 6 hours to obtain anti-aging siloxane; 1,3-bis(3-aminopropyl)tetramethyldisiloxane, anti-aging siloxane, dimethoxydimethylsilane, deionized water and 38% hydrochloric acid solution were mixed in a mass ratio of 16:70:110:500:3, stirred at 300 r / min for 35 minutes, heated to 60°C, and continued to stir for 3.5 hours, added sodium carbonate 0.05 times the mass of dimethoxydimethylsilane, continued to stir for 30 minutes, and dried at 100°C for 24 hours to obtain terminal amino polysiloxane; (2) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:11:11:28, stirred at 300 r / min for 25 h, filtered and the filtrate was dried at 38 ° C for 2 h, immersed in methyl tert-butyl ether, allowed to stand for 20 min, filtered, and vacuum dried for 25 h to obtain polyether F127 diacrylate; at 0 ° C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine were mixed in a molar ratio of 0.007:1200:105:0.45:0.8, stirred at 300 r / min for 25 min, heated to room temperature, and allowed to stand under vacuum for 26 h to obtain a self-healing gel; (3) Methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine were mixed in a molar ratio of 1:1, a catalyst in an amount of 0.05 times the mass of methyldimethoxysilane was added, and the mixture was reacted at 70°C for 6 hours to obtain a modified siloxane; (4) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:52, stirred at 90°C and 300 r / min for 30 min, cooled to room temperature, added with the diamine mixture, and continued to stir for 20 min. Then, 0.5 times the molar amount of terephthaloyl chloride of the diamine mixture and 0.06 times the volume of pyridine of N-methylpyrrolidone were added, stirred at -4°C and 1300 r / min for 25 min, heated to room temperature, and continued to stir. 35min to obtain aramid emulsion; using aramid emulsion as shell solution and self-healing gel as core solution, coaxial electrospinning was carried out, standing for 8h, and naturally cooled to room temperature to obtain pre-modified aramid fiber; modified nano-silica, modified aramid fiber and isopropanol were mixed evenly in a mass ratio of 1:8:18, stirred at 95℃, 300r / min for 7h, centrifuged to obtain solid, washed with deionized water 5 times, and dried at 100℃ for 4h to obtain modified aramid fiber; (5) Under argon protection, natural rubber, modified aramid fiber, terminal amino polysiloxane and ethanol were mixed in a mass ratio of 11:5:2:30, stirred at 55°C and 400 r / min for 5 h, vacuum dried at 70°C for 13 h, and vulcanized to obtain a modified rubber; the modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 50 h, taken out, immersed in deionized water for ultrasonication for 20 min, and dried at -1°C under vacuum conditions for 24 h to obtain a puncture-resistant inner tube.

[0022] Comparative Example 1 A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) 1,3-bis(3-aminopropyl)tetramethyldisiloxane, 3-aminopropylmethyldimethoxysilane, dimethoxydimethylsilane, deionized water and 37% hydrochloric acid solution were mixed in a mass ratio of 15:60:105:400:2, stirred at 250 r / min for 30 min, heated to 55°C, and stirred for 3 h, then added with sodium carbonate 0.04 times the mass of dimethoxydimethylsilane, stirred for 25 min, and dried at 90°C for 22 h to obtain amino-terminated polysiloxane; (2) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:10.5:10.5:27, stirred at 250 r / min for 24 h, filtered and the filtrate was dried at 37 ° C for 1.5 h, immersed in methyl tert-butyl ether, allowed to stand for 15 min, filtered, and vacuum dried for 24 h to obtain polyether F127 diacrylate; at -2 ° C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine were mixed in a molar ratio of 0.006:1150:100:0.425:0.75, stirred at 250 r / min for 20 min, heated to room temperature, and allowed to stand under vacuum for 24 h to obtain a self-healing gel; (3) Methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine were mixed in a molar ratio of 1:1, a catalyst in an amount of 0.04 times the mass of methyldimethoxysilane was added, and the mixture was reacted at 65°C for 5 hours to obtain modified siloxane; (4) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:51.5, stirred at 80°C and 250 r / min for 25 min, cooled to room temperature, added with the diamine mixture, and stirred for 15 min. Then, 0.475 times the molar amount of terephthaloyl chloride of the diamine mixture and 0.05 times the volume of pyridine of N-methylpyrrolidone were added, stirred at -5°C and 1200 r / min for 20 min, heated to room temperature, and then stirred for 15 min. The mixture was stirred for 30 min to obtain an aramid emulsion; the aramid emulsion was used as the shell solution and the self-healing gel was used as the core solution for coaxial electrospinning, and the mixture was allowed to stand for 7 h and naturally cooled to room temperature to obtain a pre-modified aramid fiber; the modified nano-silica, the modified aramid fiber and isopropanol were uniformly mixed in a mass ratio of 1:7:17, stirred at 90°C and 250 r / min for 6 h, the solid was separated by centrifugation, washed with deionized water 4 times, and dried at 95°C for 3 h to obtain the modified aramid fiber; (5) Under argon protection, natural rubber, modified aramid fiber, amino-terminated polysiloxane and ethanol were mixed in a mass ratio of 10:4:1.5:25, stirred at 50°C and 350 r / min for 4 h, vacuum dried at 65°C for 12 h, and vulcanized to obtain a modified rubber; the modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 49 h, taken out, immersed in deionized water for 15 min, and dried at -5.5°C under vacuum conditions for 23 h to obtain a puncture-resistant inner tube.

[0023] Comparative Example 2 A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:10.5:10.5:27, stirred at 250 r / min for 24 h, filtered and the filtrate was dried at 37 ° C for 1.5 h, immersed in methyl tert-butyl ether, allowed to stand for 15 min, filtered, and vacuum dried for 24 h to obtain polyether F127 diacrylate; at -2 ° C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine were mixed in a molar ratio of 0.006:1150:100:0.425:0.75, stirred at 250 r / min for 20 min, heated to room temperature, and allowed to stand under vacuum for 24 h to obtain a self-healing gel; (2) Methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine were mixed in a molar ratio of 1:1, a catalyst in an amount of 0.04 times the mass of methyldimethoxysilane was added, and the mixture was reacted at 65°C for 5 hours to obtain modified siloxane; (3) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:51.5, stirred at 80°C and 250 r / min for 25 min, cooled to room temperature, added with the diamine mixture, and stirred for 15 min. Then, 0.475 times the molar amount of terephthaloyl chloride of the diamine mixture and 0.05 times the volume of pyridine of N-methylpyrrolidone were added, stirred at -5°C and 1200 r / min for 20 min, heated to room temperature, and then stirred for 15 min. The mixture was stirred for 30 min to obtain an aramid emulsion; the aramid emulsion was used as the shell solution and the self-healing gel was used as the core solution for coaxial electrospinning, and the mixture was allowed to stand for 7 h and naturally cooled to room temperature to obtain a pre-modified aramid fiber; the modified nano-silica, the modified aramid fiber and isopropanol were uniformly mixed in a mass ratio of 1:7:17, stirred at 90°C and 250 r / min for 6 h, the solid was separated by centrifugation, washed with deionized water 4 times, and dried at 95°C for 3 h to obtain the modified aramid fiber; (4) Under argon protection, natural rubber, modified aramid fiber and ethanol were mixed in a mass ratio of 10:4:25, stirred at 50°C and 350 r / min for 4 h, vacuum dried at 65°C for 12 h, and vulcanized to obtain modified rubber; the modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 49 h, taken out, immersed in deionized water for 15 min, and dried at -5.5°C under vacuum conditions for 23 h to obtain a puncture-resistant inner tube.

[0024] Comparative Example 3 A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) 3-aminopropylmethyldimethoxysilane, salicylaldehyde and ethanol were mixed in a mass ratio of 1:1:11, reacted at 25°C and 30 r / min for 6 h, and vacuum dried at 60°C for 5 h to obtain anti-aging siloxane; 1,3-bis(3-aminopropyl)tetramethyldisiloxane, anti-aging siloxane, dimethoxydimethylsilane, deionized water and 37% hydrochloric acid solution were mixed in a mass ratio of 15:60:105:400:2, stirred at 250 r / min for 30 min, heated to 55°C, and continued to stir for 3 h, added sodium carbonate 0.04 times the mass of dimethoxydimethylsilane, continued to stir for 25 min, and dried at 90°C for 22 h to obtain terminal amino polysiloxane; (2) Under argon protection, natural rubber, modified nano-silica, terminal amino polysiloxane and ethanol were mixed in a mass ratio of 10:0.5:1.5:25, stirred at 50°C and 350 r / min for 4 h, vacuum dried at 65°C for 12 h, and vulcanized to obtain modified rubber; the modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 49 h, taken out, immersed in deionized water for 15 min, and dried at -5.5°C under vacuum conditions for 23 h to obtain a puncture-resistant inner tube.

[0025] Comparative Example 4 A method for preparing a puncture-resistant inner tube material, the method for preparing the puncture-resistant inner tube material mainly comprising the following preparation steps: (1) 3-aminopropylmethyldimethoxysilane, salicylaldehyde and ethanol were mixed in a mass ratio of 1:1:11, reacted at 25°C and 30 r / min for 6 h, and vacuum dried at 60°C for 5 h to obtain anti-aging siloxane; 1,3-bis(3-aminopropyl)tetramethyldisiloxane, anti-aging siloxane, dimethoxydimethylsilane, deionized water and 37% hydrochloric acid solution were mixed in a mass ratio of 15:60:105:400:2, stirred at 250 r / min for 30 min, heated to 55°C, and continued to stir for 3 h, added sodium carbonate 0.04 times the mass of dimethoxydimethylsilane, continued to stir for 25 min, and dried at 90°C for 22 h to obtain terminal amino polysiloxane; (2) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:10.5:10.5:27, stirred at 250 r / min for 24 h, filtered and the filtrate was dried at 37 ° C for 1.5 h, immersed in methyl tert-butyl ether, allowed to stand for 15 min, filtered, and vacuum dried for 24 h to obtain polyether F127 diacrylate; at -2 ° C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine were mixed in a molar ratio of 0.006:1150:100:0.425:0.75, stirred at 250 r / min for 20 min, heated to room temperature, and allowed to stand under vacuum for 24 h to obtain a self-healing gel; (3) Methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine were mixed in a molar ratio of 1:1, a catalyst in an amount of 0.04 times the mass of methyldimethoxysilane was added, and the mixture was reacted at 65°C for 5 hours to obtain modified siloxane; (4) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:51.5, stirred at 80°C and 250 r / min for 25 min, cooled to room temperature, added with the diamine mixture, and continued to stir for 15 min. Then, 0.475 times the molar amount of terephthaloyl chloride of the diamine mixture and 0.05 times the volume of pyridine of N-methylpyrrolidone were added, stirred at -5°C and 1200 r / min for 20 min, heated to room temperature, and continued to stir for 30 min to obtain aramid emulsion; coaxial electrospinning was carried out with the aramid emulsion as the shell solution and the self-healing gel as the core solution, and the mixture was allowed to stand for 7 h, and naturally cooled to room temperature to obtain pre-modified aramid fiber; (5) Under argon protection, natural rubber, pre-modified aramid fiber, terminal amino polysiloxane and ethanol were mixed in a mass ratio of 10:3.5:1.5:25, stirred at 50°C and 350 r / min for 4 h, vacuum dried at 65°C for 12 h, and vulcanized to obtain a modified rubber; the modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40 W purple LED lamp with a wavelength of 370 nm for 49 h, taken out, immersed in deionized water for 15 min, and dried at -5.5°C under vacuum conditions for 23 h to obtain a puncture-resistant inner tube.

[0026] Test Example 1 Puncture test Test method: Carcass strength test is used to determine the puncture resistance of tires, and the round head of the national standard round rod pressure column is changed to a cone, and the test is carried out under standard inflation pressure conditions. The results are shown in Table 1.

[0027] Table 1

[0028] From the comparison of the experimental data in Table 1, it can be found that the puncture-resistant inner tube prepared by the present invention has good puncture resistance.

[0029] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 3 in Table 1, it can be found that the materials of Examples 1, 2, 3 are not punctured compared with Comparative Example 3, which shows that the coaxial electrospinning of aramid emulsion and self-repairing gel can produce an anti-puncture material with excellent effect and enhance the anti-puncture ability of the inner tube.

[0030] Test Example 2 Durability test Test method: Use a pneumatic cutting machine to cut two 25mm dumbbell-shaped specimens into standard, test the tensile strength, put the cut specimens into a 100℃ blast hot air aging box for accelerated aging, take out the specimens after aging for 7 days, test the tensile strength again, and test the tensile retention rate, where the tensile retention rate = tensile strength after aging / tensile strength before aging*100%. The results are shown in Table 2.

[0031] Table 2

[0032] From the comparison of the experimental data in Table 2, it can be found that the puncture-resistant inner tube prepared by the present invention has good durability.

[0033] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 1 in Table 2, it can be found that the elongation-to-break retention rates of Examples 1, 2, 3 are greater than those of Comparative Example 1, which indicates that the reaction of 3-aminopropylmethyldimethoxysilane with salicylaldehyde first can generate an anti-aging structure, extend the service life of the inner tube, and increase the elongation-to-break retention rate of the material.

[0034] Test Example 3 Wear test Test method: DIN abrasion tester was used to test according to QBT-2884 standard. The results are shown in Table 3.

[0035] Table 3

[0036] From the comparison of the experimental data in Table 3, it can be found that the puncture-resistant inner tube prepared by the present invention has good wear resistance.

[0037] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 2 in Table 3, it can be found that the fracture retention rates of Examples 1, 2, 3 are greater than those of Comparative Example 2, which indicates that nano-silicon dioxide can enhance the wear resistance of the material.

[0038] Test Example 4 Flame retardant test Test method: Test the limiting oxygen index according to GB / T2406 test standard. The results are shown in Table 4 Table 4

[0039] From the comparison of the experimental data in Table 4, it can be found that the puncture-resistant inner tube prepared by the present invention has good flame retardancy.

[0040] From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 2 in Table 4, it can be found that the limiting oxygen index of Examples 1, 2, and 3 is larger than that of Comparative Example 2, which indicates that when the silicon-oxygen chain burns, the silicon-oxygen bond in the molecule will be converted into a silicon-carbon bond, and together with the generated carbonized product, a composite carbon layer is formed. This composite carbon layer has the advantages of blocking heat, isolating oxygen, and preventing molten droplets, and seals the polymer material to prevent the flammable gas from diffusing outward, thereby improving the flame retardancy of the material; From the comparison of the experimental data of Examples 1, 2, 3 and Comparative Example 3, it can be found that the limiting oxygen index of Examples 1, 2, 3 is larger than that of Comparative Example 3, which shows that the aramid fiber can decompose to produce non-combustible gas after absorbing heat. On the one hand, it can dilute the concentration of oxygen in the air and combustibles produced by thermal decomposition of the polymer. On the other hand, the nitrogen oxides produced by the decomposition can capture free radicals, thereby making the material flame retardant.

[0041] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A puncture-resistant inner tube material, characterized in that: The puncture-proof inner tube material is prepared by reacting natural rubber, modified aramid fiber, and amino-terminated polysiloxane and then modifying with a mixed solution of N-(trifluoromethylthio)phthalimide; The amino-terminated polysiloxane is prepared by first reacting 3-aminopropylmethyldimethoxysilane with salicylaldehyde and then reacting with 1,3-bis(3-aminopropyl)tetramethyldisiloxane and dimethoxydimethylsilane; The modified aramid fiber is prepared by coaxially electrospinning aramid emulsion and self-repairing gel, and then reacting with modified nano-silicon dioxide; The aramid emulsion is prepared by reacting a diamine mixture with terephthaloyl chloride; The self-repairing gel is prepared by reacting poloxamer, triethylamine, acryloyl chloride and dichloromethane and then polymerizing polyester monomers therein.

2. A method for preparing a puncture-resistant inner tube material, characterized in that: The preparation method of the puncture-resistant inner tube material mainly comprises the following preparation steps: (1) 3-aminopropylmethyldimethoxysilane, salicylaldehyde and ethanol were mixed in a mass ratio of 1:1:10-12, reacted at 24-26°C and 25-35r / min for 5-7h, and vacuum dried at 55-65°C for 4-6h to obtain anti-aging siloxane; 1,3-bis(3-aminopropyl)tetramethyldisiloxane, anti-aging siloxane, dimethoxydimethylsilane, deionized water and 36-38% hydrochloric acid solution were mixed. Mix according to the mass ratio of 14-16:50-70:100-110:300-500:1-3, stir at 200-300 r / min for 25-35 min, heat to 50-60°C, continue stirring for 2.5-3.5 h, add sodium carbonate 0.03-0.05 times the mass of dimethoxydimethylsilane, continue stirring for 20-30 min, dry at 80-100°C for 20-24 h to obtain amino-terminated polysiloxane; (2) Under nitrogen protection, poloxamer, triethylamine, acryloyl chloride and dichloromethane were mixed in a molar ratio of 1:10-11:10-11:26-28, stirred at 200-300 r / min for 23-25 ​​h, filtered to obtain the filtrate, dried the filtrate at 36-38 °C for 1-2 h, immersed in methyl tert-butyl ether, allowed to stand for 10-20 min, filtered, and vacuum dried for 23-25 ​​h to obtain polyether F127 dipropylene Acid ester; at -4~0°C, F127 diacrylate, deionized water, polyester monomer, potassium disulfate and tetramethylethylenediamine are mixed in a molar ratio of 0.005~0.007:1100~1200:95~105:0.4~0.45:0.7~0.8, stirred at 200~300r / min for 15~25min, heated to room temperature, and allowed to stand under vacuum for 22~26h to obtain a self-healing gel; (3) Mix methyldimethoxysilane and N,N'-di(3-aminopropyl)-2-butene-1,4-diamine in a molar ratio of 1:1, add a catalyst in an amount of 0.03 to 0.05 times the mass of methyldimethoxysilane, and react at 60 to 70°C for 4 to 6 hours to obtain modified siloxane; (4) Under nitrogen protection, calcium chloride and N-methylpyrrolidone were mixed in a mass ratio of 1:51~52, stirred at 70~90℃ and 200~300r / min for 20~30min, cooled to room temperature, added with diamine mixture, continued stirring for 10~20min, added with 0.45~0.5 times the molar amount of amino group in the diamine mixture of terephthaloyl chloride and 0.04~0.06 times the volume of N-methylpyrrolidone of pyridine, stirred at -6~-4℃ and 1100~1300r / min for 15~25min, heated to room temperature, continued stirring for 25~35min, and obtained aramid emulsion; coaxial electrospinning was carried out with aramid emulsion as shell solution and self-healing gel as core solution, left to stand for 6~8h, and naturally cooled to room temperature to obtain pre-modified aramid fiber; The modified nano-silica, modified aramid fiber and isopropanol are uniformly mixed in a mass ratio of 1:6-8:16-18, stirred at 85-95°C and 200-300 r / min for 5-7 hours, centrifuged to obtain a solid, washed with deionized water for 3-5 times, and dried at 90-100°C for 2-4 hours to obtain the modified aramid fiber; (5) Under argon protection, natural rubber, modified aramid fiber, amino-terminated polysiloxane and ethanol are mixed in a mass ratio of 9-11:3-5:1-2:20-30, stirred at 45-55°C and 300-400 r / min for 3-5 h, vacuum dried at 60-70°C for 11-13 h, and vulcanized to obtain a modified rubber; The modified rubber was immersed in a mixed solution of N-(trifluoromethylthio)phthalimide, placed in a closed photoreactor under nitrogen protection, irradiated with a 40W purple LED lamp with a wavelength of 370nm for 48-50 hours, taken out, immersed in deionized water for 10-20 minutes of ultrasound, and dried at -10--1°C under vacuum conditions for 22-24 hours to obtain a puncture-resistant inner tube.

3. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The polyester monomer in step (2) is prepared by uniformly mixing methyl methacrylate, 4-vinylbenzene boronic acid and 3-butene-1,2-diol in a molar ratio of 4-6:1:

1.

4. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The catalyst in step (3) is prepared by uniformly mixing chloroplatinic acid and isopropanol in a mass ratio of 1:75-82.

5. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The modified nano-silica in step (4) is prepared by uniformly mixing nano-silica, 3-aminopropyltrimethoxysilane and isopropanol in a mass ratio of 1:1:6-8, stirring at 85-95°C and 200-300 r / min for 5-7 hours, centrifuging to obtain a solid, washing it with deionized water for 3-5 times, and drying it at 90-100°C for 2-4 hours.

6. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The diamine mixture in step (4) is prepared by uniformly mixing m-phenylenediamine, p-phenylenediamine and modified siloxane in a molar ratio of 0.5-0.6:1:0.1-0.

2.

7. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The liquid flow rate of the shell solution in step (4) is 0.9-1.1 ml / h.

8. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The liquid flow rate of the core solution in step (4) is 0.2-0.3 ml / h.

9. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The vulcanization in step (5) is carried out on a flat vulcanizing press with the following parameters: the size of the upper and lower heating plates is 30 cm×30 cm, the temperature range of the upper platen of the press is 0~300°C, the temperature range of the lower platen is 0~300°C, and the pressure range of the press is 0~40MPa.

10. The method for preparing a puncture-resistant inner tube material according to claim 2, characterized in that: The N-(trifluoromethylthio)phthalimide mixed solution in step (5) is prepared by uniformly mixing N-(trifluoromethylthio)phthalimide, acetonitrile and benzophenone in a mass ratio of 7-8:0.5-1:49-53.

Citation Information

Patent Citations

  • Modified para-aramid stock solution as well as preparation method and application thereof

    CN114316257A

  • Heat-resistant inner tube material and preparation method thereof

    CN118725477A

  • Heat-stable inner tube material and preparation method thereof

    CN118755159A