Crosslinked polyethylene insulating material for ultrahigh-voltage cable and preparation method of crosslinked polyethylene insulating material
By using low-density polyethylene, antioxidants and composite crosslinking agents in high-voltage DC cables, the insulating materials with high crosslinking density and crystallinity are solved, and the problem of low space charge accumulation and production efficiency is improved, and the resistance of the cable is improved Breakdown performance and production efficiency.
Patent Information
- Application Number
- CN202411325184.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-23
AI Technical Summary
Crosslinked polyethylene insulating materials in high-voltage DC cables will accumulate space charge under the action of high-voltage DC for a long time, resulting in distortion and breakdown of electric field distribution in the insulating layer. In the prior art, the high amount of crosslinking agents will lead to low production efficiency and high cost.
Low-density polyethylene is used as the main component, and antioxidants and composite crosslinking agents are added to form a specific crosslinking network and prepared by antioxidants, reducing the amount of crosslinking agent, improving crosslinking density and crystallinity, and inhibiting space charge accumulation. And the material's migration resistance and hydrolysis resistance are improved through the multi-ring conjugated structure of the antioxidant.
The breakdown voltage level of the cable is improved, the space charge aggregation and the existence of amorphous areas of the electric tree are reduced, the oxidation induction time is extended, and the breakdown resistance and production efficiency of the insulating material are improved.
Smart Images

Figure BDA0005055221570000071 
Figure BDA0005055221570000081
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cable materials, and in particular relates to a cross-linked polyethylene insulating material for an ultra-high voltage cable and a preparation method thereof. Background Art
[0002] With the development of ocean and the advancement of new urbanization, more and more high-voltage DC cable projects are put into operation. The role of the insulating material in the cable is to cover the outside of the conductive material, prevent current leakage, and ensure the safety and reliability of the cable during transmission. In recent years, extruded insulated cables have become the mainstream technology of high-voltage DC cables due to their advantages such as short production cycle, low environmental impact, and easy installation and maintenance.
[0003] Extruded insulated cables mainly include polypropylene thermoplastic elastomer insulated cables and polyethylene insulated cables. Among them, cross-linked polyethylene insulation materials have the advantages of excellent insulation performance, simple laying, and convenient maintenance. At present, they have become the absolute mainstream of cables in my country. In industrial applications, cross-linked polyethylene mainly includes silane cross-linking method, peroxide cross-linking method, irradiation cross-linking method and ultraviolet light cross-linking method that has emerged in recent years. Among them, peroxide cross-linking method is widely used in the insulation cross-linking of current medium-high voltage and ultra-high voltage power cables due to its less restrictiveness.
[0004] However, when the cross-linked polyethylene used in high-voltage DC cables is exposed to high-voltage DC for a long time, a large amount of space charge will accumulate inside, which will cause the electric field distribution inside the insulation layer to be distorted and even to break down. Patent CN 115651105B discloses a grafted modified cross-linked polyethylene water-tree resistant insulation material and its preparation method and application, which uses a two-step blending method to reduce the pore defects inside the insulation material and effectively improve the water-tree resistant performance and electrical properties of the material. However, although the first step of this method uses less DCP cross-linking agent to reduce the gel caused by the cross-linking of low-density polyethylene itself, in the second step of cross-linking, in order to ensure the high cross-linking degree of the insulation material, the cross-linking agent content is usually added at a high level, so that when extruded for a long time, too much cross-linking agent will decompose to produce pre-cross-linking or old glue points, which reduces the cable insulation extrusion production cycle and production efficiency, and causes a large amount of production waste, increasing the cable production cost. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention selects low-density polyethylene as the main component, adds an antioxidant and a composite cross-linking agent, and ensures the purity of the insulating material to the greatest extent, prepares and synthesizes a cross-linked polyethylene insulating material for ultra-high voltage cables, and improves the breakdown voltage level of the cable.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The first aspect of the present invention provides a cross-linked polyethylene insulation material for ultra-high voltage cables, which comprises the following raw materials in parts by weight: 70 to 100 parts of low-density polyethylene, 0.4 to 1.2 parts of an antioxidant and 1.5 to 5.5 parts of a composite cross-linking agent; wherein the antioxidant contains a polycyclic conjugated structure.
[0008] The higher the voltage level of the power cable, the easier it is for insulation breakdown to occur, thus leading to insulation failure. Therefore, the higher the voltage level of the power cable, the higher the requirements for the purity and impurity content of the insulation material. In this regard, the basic components of the insulation material of the present application are pure polyethylene, a cross-linking agent and an antioxidant, which ensures the purity of the insulation material to the greatest extent.
[0009] In some embodiments, the low density polyethylene has a melt flow index of 1.0 to 3.0 g / 10 min at 190° C. and 2.16 kg.
[0010] The present application increases the probability of cross-linking network formation in the early stages of cross-linking network formation through the specific selection of low-density polyethylene, thereby reducing the amount of cross-linking agent used. However, the early easy cross-linking will also cause the molecules to entangle together, resulting in a decrease in the cross-linking sites between molecules and a decrease in the cross-linking density.
[0011] In some embodiments, the composite cross-linking agent comprises dicumyl peroxide, di-tert-butylcumyl peroxide, and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane.
[0012] In some embodiments, the mass ratio of dicumyl peroxide, di-tert-butyl cumene peroxide and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane is 1:(0.33-0.39):(0.17-0.26).
[0013] The present application reduces the amount of cross-linking agent used by compounding the cross-linking agent. The different decomposition rates of the cross-linking agent make the free radical generation rate more gradual, improve the crystal structure inside the polyethylene, increase the crystallinity, reduce the presence of amorphous regions that are prone to forming electric trees, and the perfect crystal structure helps to reduce the accumulation of space charges and accelerate the heat dissipation process.
[0014] However, after high-temperature decomposition of diisopropylbenzene peroxide, substances such as acetophenone, methane, and cumyl alcohol will be produced; di-tert-butyl peroxide isopropylbenzene will also produce byproducts such as aromatic diols and aromatic diketones. In the ordinary processing of cables, a small part of these cross-linked byproducts escape under high temperature, and most of them stay in the impenetrable gaps or attach to the polymer chains. After the cable is powered on, it slowly escapes from the insulation layer to form insulating pores, which brings safety hazards. The cross-linking density of polyethylene in the early stage of this application is low, which can promote the discharge of some byproducts.
[0015] In some embodiments, the preparation steps of the antioxidant are as follows:
[0016] S1. Under the protection of inert gas, stir resorcinol, fatty aldehyde, hydrochloric acid and anhydrous ethanol at 60-80°C for 8-14 hours, cool to room temperature, wash, recrystallize 1-2 times with acetone-n-hexane solution, and vacuum dry at 40-60°C to constant weight to obtain a white powder;
[0017] S2, dissolving the white powder of step S1 in acetone-n-hexane solution, passing inert gas, and simultaneously adding β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl chloride-n-hexane solution and triethylamine-n-hexane solution at 1-4°C, stirring for 20-40 minutes after the addition is completed, heating to 30-50°C, and keeping warm for 18-30 hours. After the insulation is completed, first rotary evaporation, then adding toluene and stirring, and then filtering and continuing rotary evaporation to obtain a crude product;
[0018] S3, adding the crude product obtained in step S2 dropwise into icy ether at a rotation speed of 400-600 rpm, and after the addition is completed, standing, suction filtering, washing, and vacuum drying at 25-35° C. to constant weight to obtain the antioxidant.
[0019] Cross-linked polyethylene is the most commonly used main insulation for high-voltage cables. Antioxidants are usually added to the industry to improve its processing characteristics and long-term electrical properties. In actual applications, the molecular weight of traditional antioxidants is generally relatively small. During processing and use, they have defects such as poor thermal stability, high volatility and low migration resistance, which makes the antioxidants fail to achieve the expected antioxidant effect and thus cannot inhibit or slow down the aging of polymer materials. Some commercial macromolecular antioxidants have the problem of limited antioxidant performance due to poor fusion with cross-linked polyethylene.
[0020] The antioxidant of the present application has a multi-ring conjugated structure, which makes it non-volatile, migration-resistant and hydrolysis-resistant during use, meeting the processing requirements of cross-linked polyethylene materials; on the second hand, the cross-linked polyethylene added with the antioxidant can effectively inhibit the accumulation of space charge, alleviate the local electric field distortion in the polymer caused by the continuous accumulation of space charge during the use of the cable, and thus improve the breakdown resistance of the insulating material. The possible reason is that the antioxidant changes the crystal morphology of the cross-linked polyethylene and reduces the formation of grain boundary defects, or the dipole charge center of the strong polar group in the antioxidant leads to the generation of traps, which binds the movable charge in the material and prevents it from accumulating in large quantities under the influence of the electric field, thereby inhibiting the generation of space charge; on the third hand, since peroxide cross-linking mainly controls its cross-linking degree through heating temperature, when the cross-linking degree is not appropriate, the heat resistance of the cross-linked polyethylene is poor and cannot meet the requirements for long-term use of the cable, and the antioxidant of the present application will undergo electron migration during the cross-linking process to generate a relatively stable structure, thereby increasing the oxidation induction time and the oxidation starting temperature.
[0021] In some embodiments, the carbon chain length of the fatty aldehyde in step S1 is C8-C16.
[0022] In some embodiments, the molar ratio of resorcinol to fatty aldehyde in step S1 is 1:(1.05-1.3).
[0023] In some embodiments, the mass ratio of the white powder to β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride in step S2 is 1:(2.15-2.35).
[0024] In some embodiments, the mass ratio of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride to triethylamine in step S2 is 1:(0.3-0.4).
[0025] The second aspect of the present invention provides a method for preparing a cross-linked polyethylene insulation material for ultra-high voltage cables, comprising the following steps: mixing and extruding low-density polyethylene, an antioxidant and a composite cross-linking agent at 110-130°C to obtain the cross-linked polyethylene insulation material for ultra-high voltage cables.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The basic components of the insulating material of the present invention are pure polyethylene, a cross-linking agent and an antioxidant, which ensures the purity of the insulating material to the greatest extent, has a good ability to inhibit the accumulation of space charges, and improves the withstand voltage level of the cable.
[0028] 2. The present application reduces the amount of cross-linking agent used and improves the crystalline structure inside the polyethylene by compounding the cross-linking agent, which not only reduces the presence of amorphous regions that are prone to forming electrical trees, but also helps to reduce the accumulation of space charges and accelerate the heat dissipation process.
[0029] 3. The cross-linking density of the polyethylene of the present invention is relatively low in the early stage, which promotes the discharge of a part of the cross-linking agent by-products and improves the cross-linking density in the later stage.
[0030] 4. The antioxidant of the present application is not easy to volatilize, is resistant to migration and hydrolysis during use, can increase the oxidation induction time and oxidation starting temperature, meet the processing requirements of cross-linked polyethylene materials, and can effectively inhibit the accumulation of space charges, thereby improving the breakdown resistance of insulating materials. DETAILED DESCRIPTION
[0031] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0032] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments are described as follows:
[0033] Low-density polyethylene was purchased from Sinopec Beijing Yanshan Branch, with a melt flow index of 2.0 g / 10 min (190 ° C, 2.16 kg) and a density of 0.915 g / cm 3 .
[0034] Preparation Example 1
[0035] The preparation steps of Antioxidant-A are as follows:
[0036] S1. Under nitrogen protection, 100 g of resorcinol, 212 g of lauryl aldehyde, 140 mL of 20 wt% hydrochloric acid and 960 mL of anhydrous ethanol were stirred at 70° C. for 10 h, cooled to room temperature, then washed with anhydrous ethanol 3 times, then recrystallized with 50 v% acetone-n-hexane solution 2 times, and vacuum dried at 50° C. to constant weight to obtain a white powder;
[0037] S2, dissolving 50g of the white powder of step S1 in 1000mL of 50v% acetone-n-hexane solution, passing nitrogen, and simultaneously adding dropwise 112.5g of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride-800mL of n-hexane solution and 39.4g of triethylamine-470mL of n-hexane solution at 2°C, stirring for 30min after the addition is complete, heating to 40°C, and keeping warm for 25h. After the insulation is completed, first rotary evaporation, then adding toluene and stirring until precipitation occurs, and continuing rotary evaporation to constant weight after suction filtration to obtain a crude product;
[0038] S3. Add the crude product obtained in step S2 dropwise into 5 times the mass of icy ether at a rotation speed of 500 rpm. After the addition is completed, let it stand until the precipitation is complete, filter it with suction, wash it twice with icy ether, and vacuum dry it at 30°C to constant weight to obtain antioxidant-A.
[0039] Preparation Example 2
[0040] The preparation steps of Antioxidant-B are as follows:
[0041] The difference between this preparation example and preparation example 1 is that in step S1, 168 g of lauryl aldehyde is replaced by 115 g of hexanal.
[0042] Preparation Example 3
[0043] The preparation steps of Antioxidant-C are as follows:
[0044] The difference between this preparation example and preparation example 1 is that 168 g of lauryl aldehyde in step S1 is replaced by 308 g of stearic aldehyde.
[0045] Preparation Example 4
[0046] The preparation steps of Antioxidant-D are as follows:
[0047] The difference between this preparation example and preparation example 1 is that the amount of lauryl aldehyde used in step S1 is 184 g.
[0048] Preparation Example 5
[0049] The preparation steps of Antioxidant-E are as follows:
[0050] The difference between this preparation example and preparation example 1 is that the amount of lauryl aldehyde used in step S1 is 248 g.
[0051] Preparation Example 6
[0052] The preparation steps of Antioxidant-F are as follows:
[0053] The difference between this preparation example and preparation example 1 is that the amount of white powder used in step S2 is 45 g.
[0054] Preparation Example 7
[0055] The preparation steps of Antioxidant-G are as follows:
[0056] The difference between this preparation example and preparation example 1 is that the amount of white powder used in step S2 is 55 g.
[0057] Example 1
[0058] A cross-linked polyethylene insulation material for ultra-high voltage cables, comprising the following raw materials by weight: 85 parts of low-density polyethylene, 0.8 parts of antioxidant-A and 3.5 parts of composite cross-linking agent;
[0059] The composite crosslinking agent comprises 2.2 parts of dicumyl peroxide, 0.8 parts of di-tert-butyl cumyl peroxide and 0.5 parts of 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane;
[0060] The preparation method of cross-linked polyethylene insulation material for ultra-high voltage cable in this embodiment comprises the following steps: low-density polyethylene, antioxidant-A, diisopropylbenzene peroxide, di-tert-butyl peroxide isopropylbenzene and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane are mixed and extruded at 120° C. to obtain cross-linked polyethylene insulation material for ultra-high voltage cable.
[0061] Example 2
[0062] A cross-linked polyethylene insulation material for ultra-high voltage cables, comprising the following raw materials, by weight: 70 parts of low-density polyethylene, 0.4 parts of antioxidant-A and 1.5 parts of a composite cross-linking agent;
[0063] The composite crosslinking agent comprises 1 part of dicumyl peroxide, 0.33 parts of di-tert-butyl cumyl peroxide and 0.17 parts of 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane;
[0064] The preparation method of the cross-linked polyethylene insulation material for ultra-high voltage cable in this embodiment comprises the following steps: low-density polyethylene, antioxidant-A, diisopropylbenzene peroxide, di-tert-butyl peroxide isopropylbenzene and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane are mixed and extruded at 110° C. to obtain the cross-linked polyethylene insulation material for ultra-high voltage cable.
[0065] Example 3
[0066] A cross-linked polyethylene insulation material for ultra-high voltage cables, comprising the following raw materials, by weight: 100 parts of low-density polyethylene, 1.2 parts of antioxidant-A and 5.5 parts of composite cross-linking agent;
[0067] The composite crosslinking agent comprises 3.3 parts of dicumyl peroxide, 1.29 parts of di-tert-butyl cumyl peroxide and 0.91 parts of 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane;
[0068] The preparation method of the cross-linked polyethylene insulation material for ultra-high voltage cables in this embodiment comprises the following steps: low-density polyethylene, antioxidant-A, diisopropylbenzene peroxide, di-tert-butyl peroxide isopropylbenzene and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane are mixed and extruded at 130° C. to obtain the cross-linked polyethylene insulation material for ultra-high voltage cables.
[0069] Example 4
[0070] This embodiment provides a cross-linked polyethylene insulation material for ultra-high voltage cables and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that antioxidant-A is replaced by an equal portion of antioxidant-B.
[0071] Example 5
[0072] This embodiment provides a cross-linked polyethylene insulation material for ultra-high voltage cables and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that antioxidant-A is replaced by an equal portion of antioxidant-C.
[0073] Example 6
[0074] This embodiment provides a cross-linked polyethylene insulation material for ultra-high voltage cables and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that antioxidant-A is replaced by an equal portion of antioxidant-D.
[0075] Example 7
[0076] This embodiment provides a cross-linked polyethylene insulation material for ultra-high voltage cables and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that antioxidant-A is replaced by an equal portion of antioxidant-E.
[0077] Example 8
[0078] This embodiment provides a cross-linked polyethylene insulation material for ultra-high voltage cables and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that antioxidant-A is replaced by an equal portion of antioxidant-F.
[0079] Example 9
[0080] This embodiment provides a cross-linked polyethylene insulation material for ultra-high voltage cables and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that antioxidant-A is replaced by an equal portion of antioxidant-G.
[0081] Example 10
[0082] A cross-linked polyethylene insulation material for ultra-high voltage cables, comprising the following raw materials by weight: 85 parts of low-density polyethylene, 0.8 parts of antioxidant-A and 3.5 parts of composite cross-linking agent;
[0083] The composite crosslinking agent comprises 2.5 parts of dicumyl peroxide and 1 part of di-tert-butyl cumyl peroxide;
[0084] The preparation method of the cross-linked polyethylene insulation material for ultra-high voltage cables in this embodiment is the same as that in Example 1.
[0085] Embodiment 11
[0086] A cross-linked polyethylene insulation material for ultra-high voltage cables, comprising the following raw materials by weight: 85 parts of low-density polyethylene, 0.8 parts of antioxidant-A and 3.5 parts of composite cross-linking agent;
[0087] The composite crosslinking agent comprises 2.7 parts of dicumyl peroxide and 0.8 parts of 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane;
[0088] The preparation method of the cross-linked polyethylene insulation material for ultra-high voltage cables in this embodiment is the same as that in Example 1.
[0089] Performance Test:
[0090] 1. Gel content test:
[0091] Take 0.3g of the cross-linked polyethylene insulation material of each embodiment, record its mass as m1, wrap it with a 120-mesh copper mesh, immerse it in a xylene solution, extract it with a reflux extractor at 160°C for 4h, take out the sample, rinse it with anhydrous ethanol 3 times, and then place it in a vacuum drying oven at 100°C to dry to constant weight, weigh the mass of the cross-linked polyethylene insulation material after drying, record it as m2, and calculate the gel content (C gel ), C gel =(m2 / m1)×100%, the gel content represents the degree of cross-linking of polyethylene.
[0092] 2. DC breakdown test:
[0093] The DC breakdown field strength of the cross-linked polyethylene insulation material of each embodiment at 50° C. was measured. During the measurement, the voltage was increased at a rate of 1000 V / s by a uniform voltage increase until the sample was broken down, and the breakdown voltage was recorded.
[0094] The results are shown in Table 1.
[0095] Table 1 Performance test results
[0096]
[0097]
[0098] It can be seen from the data in Table 1 that the cross-linked polyethylene insulation materials of Examples 1-3 have high gel content and high DC breakdown voltage, indicating that their cross-linking degree and withstand voltage level are relatively high.
[0099] Compared with Example 1, in Example 4-5, the carbon chain length of the fatty aldehyde is changed when preparing the antioxidant, which is not conducive to the entanglement between the fatty aldehyde and the polyethylene, affects the fusion of the antioxidant and the cross-linked polyethylene, and further affects the cross-linking degree and pressure resistance grade of the polyethylene.
[0100] Compared with Example 1, Examples 6-9 change the dosage ratio of the raw materials when preparing the antioxidant, which is not conducive to the formation of the polycyclic conjugated structure of the antioxidant, affects the migration resistance and inhibition of space charge accumulation of the antioxidant during processing and use, and reduces the crosslinking degree and voltage resistance grade of the polyethylene.
[0101] It can be seen from Example 1 and Examples 10-11 that the compounding of three cross-linking agents can effectively increase the gel content; and the compounded cross-linking agent improves the internal crystalline structure of polyethylene, helps to reduce the accumulation of space charges, and thus improves the breakdown voltage level.
[0102] The embodiments described above do not impose any form of limitation on the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A cross-linked polyethylene insulation material for ultra-high voltage cables, characterized in that: The invention comprises the following raw materials by weight: 70 to 100 parts of low-density polyethylene, 0.4 to 1.2 parts of antioxidant and 1.5 to 5.5 parts of composite cross-linking agent; wherein the antioxidant contains a polycyclic conjugated structure.
2. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 1, characterized in that: The low-density polyethylene has a melt flow index of 1.0 to 3.0 g / 10 min at 190° C. and 2.16 kg.
3. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 1, characterized in that: The composite cross-linking agent comprises dicumyl peroxide, di-tert-butylcumyl peroxide and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane.
4. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 3, characterized in that: The mass ratio of dicumyl peroxide, di-tert-butyl cumyl peroxide and 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane is 1:(0.33-0.39):(0.17-0.26).
5. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 1, characterized in that: The preparation steps of the antioxidant are as follows: S1. Under the protection of inert gas, stir resorcinol, fatty aldehyde, hydrochloric acid and anhydrous ethanol at 60-80°C for 8-14 hours, cool to room temperature, wash, recrystallize 1-2 times with acetone-n-hexane solution, and vacuum dry at 40-60°C to constant weight to obtain a white powder; S2, dissolving the white powder of step S1 in acetone-n-hexane solution, passing inert gas, and simultaneously adding β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl chloride-n-hexane solution and triethylamine-n-hexane solution at 1-4°C, stirring for 20-40 minutes after the addition is completed, heating to 30-50°C, and keeping warm for 18-30 hours. After the insulation is completed, first rotary evaporation, then adding toluene and stirring, and then filtering and continuing rotary evaporation to obtain a crude product; S3, adding the crude product obtained in step S2 dropwise into icy ether at a rotation speed of 400-600 rpm, and after the addition is completed, standing, suction filtering, washing, and vacuum drying at 25-35° C. to constant weight to obtain the antioxidant.
6. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 5, characterized in that: The carbon chain length of the fatty aldehyde in step S1 is C8-C16.
7. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 5, characterized in that: In step S1, the molar ratio of resorcinol to fatty aldehyde is 1:(1.05-1.3).
8. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 5, characterized in that: The mass ratio of the white powder to β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride in step S2 is 1:(2.15-2.35).
9. The cross-linked polyethylene insulation material for ultra-high voltage cable according to claim 5, characterized in that: In the step S2, the mass ratio of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl chloride to triethylamine is 1:(0.3-0.4).
10. A method for preparing a cross-linked polyethylene insulation material for an ultra-high voltage cable according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing and extruding low-density polyethylene, an antioxidant and a composite cross-linking agent at 110-130° C. to obtain the cross-linked polyethylene insulation material for the ultra-high voltage cable.
Citation Information
Patent Citations
Scorch-resistant chemically-crosslinked polyethylene insulation material with high crosslinking degree and preparation method of scorch-resistant chemically-crosslinked polyethylene insulation material
CN109370003A
High-voltage ultra-clean insulating material with excellent anti-aging performance and preparation method of high-voltage ultra-clean insulating material