Flame-retardant polymer core material for aluminum composite plate and preparation method of flame-retardant polymer core material
By using layered metal-polymer combination flame retardants and other additives in aluminum composite sheet core materials, the problems of flammability and poor bonding of existing core materials have been solved, and the flame retardant effect and processing performance have been improved. Ensures building safety and productivity.
Patent Information
- Application Number
- CN202411350390.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The core materials of existing aluminum composite panels are flammable, and the flame retardant compatibility is poor, resulting in poor bonding and fire spread, and insufficient processing performance, affecting production efficiency and product quality.
The layered metal-polymer combination flame retardant prepared from pentaerythritol, phosphorus oxychloride, 4,4'-dihydroxydiphenylsulfone, zinc nitrate hexahydrate and magnesium nitrate hexahydrate, combined with antioxidants, Lubricants and tougheners form flame retardant polymer core materials with high oxygen index, and catalyze into carbon by dehydration and heat absorption of metal layers and phosphoric acid, improving flame retardant properties and bonding firmness.
The aluminum composite board core material with good flame retardant effect, firm bonding and easy to process is achieved, which reduces the combustion speed and smoke output, prevents the spread of flames, and ensures the continuous and quality stability of production.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the field of flame retardancy, and specifically relates to a flame retardant polymer core material for an aluminum composite plate and a preparation method thereof. Background Art
[0002] Aluminum composite panel is a curtain wall material and decorative material commonly used in modern buildings. It has the characteristics of light weight, beautiful appearance, high rigidity, etc. Its production process is mainly divided into hot pasting and cold pasting. The hot pasting process is to bond the core layer and the aluminum panel through the laminated polymer film melted under high temperature and high pressure, and then cool and shape to obtain the aluminum-plastic composite panel. This process can maintain continuous production, high degree of automation, and good product quality stability. It is currently adopted by most domestic companies; the cold pasting process mainly uses glue as an adhesive. It is not heated during the composite process and needs to be pressurized for a period of time for the adhesive material to solidify. This process is simple to operate, but the production efficiency is low and the product quality is unstable. At present, only a few companies with smaller production scales adopt it. The production processes of the above two aluminum composite panels mostly use polyethylene, which is easy to process and shape, as the core material, but the ordinary polyethylene oxygen index is low, which makes it flammable, and the molten drippings produced during combustion can easily ignite other items, causing the fire to spread.
[0003] At present, with the increasing emphasis on building safety, the development of flame-retardant core materials and the improvement of the flame retardancy of aluminum composite panels have become the focus of attention. For example, patent CN114989513B discloses a halogen-free environmentally friendly flame-retardant polyethylene material and a preparation method, which is obtained by blending and modifying a new NPB halogen-free environmentally friendly flame retardant made of phenylboric acid, triethanolamine and phosphorus trichloride with polyethylene to obtain an environmentally friendly flame-retardant polyethylene material. Although the polyethylene material can improve the flame retardancy of the aluminum composite panel when applied to the aluminum composite panel, the new flame retardant molecules are relatively small for the aluminum composite panel, and may migrate to the polyethylene surface, causing the bonding between the polyethylene and the aluminum surface to be slowly destroyed, resulting in debonding and poor bonding. Patent CN108912445B enhances the compatibility of flame retardants with PE by directly bonding the synthesized single-molecule reactive IFR to the PE chain, solving the problems of poor compatibility between flame retardants and substrates, easy precipitation, easy moisture absorption, poor thermal stability, and poor anti-migration. It also improves the flame retardant efficiency through the synergistic flame retardant effect of silicon compounds. However, this method uses a large amount of flame retardant-related substances, which may affect the processing performance of polyethylene.
[0004] Therefore, there is an urgent need in the market for a polyethylene material with good flame retardancy, strong bonding and easy processing as the core material of aluminum composite panels. Summary of the invention
[0005] In order to overcome the deficiencies of the above-mentioned prior art, the present invention provides a flame retardant polymer core material for aluminum composite panels and a preparation method thereof. The polymer core material has the advantages of good flame retardancy, strong bonding and easy processing, and meets the requirements of building safety.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is:
[0007] The first aspect of the present invention provides a flame retardant polymer core material for an aluminum composite plate, which comprises the following raw materials in parts by weight: 95-105 parts of polyethylene, 15-25 parts of a flame retardant, 1-4 parts of an antioxidant, 2-4 parts of a lubricant, and 2-5 parts of a toughening agent; wherein the flame retardant is a layered metal-polymer composition.
[0008] The flame retardant polymer core material of the present invention has a high oxygen index, a slow burning speed and slight smoke generation when ignited, and the flame retardant contained in it absorbs heat and dehydrates at high temperature to take away the generated combustion heat, and the oxides generated by dehydration will form a dense flame retardant barrier on the surface of the polymer core material, reducing the burning speed and the melting dripping phenomenon, thereby achieving the purpose of inhibiting combustion and preventing the spread of flames.
[0009] In some embodiments, the flame retardant is prepared by the following steps:
[0010] S1, stirring pentaerythritol and phosphorus oxychloride for 5-7 hours, purifying, and obtaining reactant 1;
[0011] S2, stirring the reactant 1 obtained in step S1 and 4,4'-dihydroxydiphenyl sulfone at 75-85° C. for 7-9 hours, washing, rotary evaporating and drying after the stirring, to obtain reactant 2;
[0012] S3, zinc nitrate hexahydrate, reactant 2 obtained in step S2 and anhydrous ethanol are stirred at room temperature for 1-3 hours, and then magnesium nitrate hexahydrate-anhydrous ethanol solution is added and stirred for 1-2 hours, followed by adding ammonia water and stirring for 1-3 hours, and then the temperature is raised to 40-60° C. and stirred for 8-16 hours, filtered, washed and dried to obtain the flame retardant.
[0013] In some embodiments, the molar ratio of pentaerythritol to phosphorus oxychloride in step S1 is 1:(2.4-3.6).
[0014] In some embodiments, the molar ratio of reactant 1 to 4,4'-dihydroxydiphenyl sulfone in step S2 is 1:(1.05-1.25).
[0015] In some embodiments, the mass ratio of zinc nitrate hexahydrate, reactant 2 and magnesium nitrate hexahydrate in step S3 is (0.38-0.52):1:(0.23-0.37).
[0016] The present invention prepares a flame retardant composed of a metal layer and a polymer, which has the following advantages: first, the thermal decomposition region of the polymer in the flame retardant covers the thermal degradation temperature range of the matrix polyethylene, broadens the temperature range of the dehydration endothermic reaction of the metal layer, so that the flame retardant can inhibit the combustion of the polymer material in a wider temperature range, which is conducive to the flame retardant to fully exert its effectiveness during the combustion process;
[0017] Secondly, when facing combustion, the phosphoric acid released by the breakage of flame retardant molecules can promote the dehydration and carbonization of flame retardants, and can also release active factors such as PO· in the gas phase to terminate the free radical reaction; and the released volatile substances reduce the contact between polyethylene and oxygen, forming a fluffy black solid; in addition, the sulfur element contained in the molecule can accelerate the collective isomerization of macromolecules to produce a large amount of CO2, promoting the cyclization of the matrix into carbon;
[0018] Thirdly, the flame retardant of the present invention improves the compatibility between the flame retardant and the polyethylene matrix through the combination of the metal layer and the polymer, so that the flame retardant is more fully coated by the matrix resin, thereby reducing the diffusion of thermal decomposition products during combustion, so that the oxides after the decomposition of the flame retardant can be more closely attached to the resin matrix to block heat propagation;
[0019] Fourthly, the metal layer in the flame retardant of the present invention has excellent catalytic carbonization ability, which makes it show faster carbon layer formation speed and stronger self-extinguishing property when burning, but the catalytically generated carbon layer is unstable and easily leads to increased smoke generation.
[0020] In some embodiments, the lubricant comprises polyethylene wax and microcrystalline wax.
[0021] Preferably, the mass ratio of the polyethylene wax to the microcrystalline wax is 1:(0.22-0.35).
[0022] In the actual production process, the inventor found that the fluidity of the core material was poor, which affected the composite effect in the thermal paste production process, increased the scrap rate, and could not maintain continuous production. To this end, the present invention enhances the fluidity of the core material through the specific selection of lubricants, making it easy to process and ensuring continuous large-scale production.
[0023] In some embodiments, the antioxidant is one or more of a hindered phenol antioxidant, a phosphite antioxidant, and a thio antioxidant.
[0024] Preferably, the antioxidant is 168 or 626.
[0025] In some embodiments, the toughening agent is ethylene-octene copolymer or maleic anhydride grafted EVA.
[0026] Preferably, the toughening agent is ethylene-octene copolymer.
[0027] Since the thermal bonding process uses the molten laminated polymer film as a glue layer to bond the core layer and the aluminum panel, the small molecule antioxidant used in the present invention may slowly destroy the glue layer during long-term use, resulting in debonding and poor bonding. In this regard, the specially selected toughening agent added in the present invention not only further improves the processing performance of the core material, but also reduces the precipitation of the small molecule antioxidant during long-term use, so that the core material and the aluminum panel are firmly bonded.
[0028] In some embodiments, the raw material further comprises 2-6 parts by weight of distilled water.
[0029] The dimethicone used in the present invention decomposes into cumene free radicals at high temperature, and the free radicals form p-π conjugation with the large π bond on the benzene ring, and have a hyperconjugation effect of two methyl groups, so that the carbon layer structure is more stable, and the problem of increased smoke generation caused by the unstable carbon layer generated by the catalysis of the flame retardant is solved. In addition, the cumene free radicals can also capture the hydroxyl free radicals generated by combustion, making it difficult for the chain reaction of combustion to proceed, thereby improving the flame retardant performance of the material.
[0030] The second aspect of the present invention provides a method for preparing a flame retardant polymer core material for an aluminum composite plate, comprising the following steps: mixing polyethylene, a flame retardant, an antioxidant, a lubricant and a toughening agent at 80-90°C for 10-20 minutes to obtain the flame retardant polymer core material for the aluminum composite plate.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The present invention provides a flame retardant polymer core material for aluminum composite panels with slow burning speed and light smoke generation. The core material has the advantages of good flame retardant effect, strong bonding with aluminum panels and easy processing.
[0033] 2. The present invention provides a flame retardant composed of a metal layer and a polymer, which can inhibit the combustion of a core material within a wide temperature range, which is conducive to fully exerting the flame retardant effect; and the metal layer in the flame retardant has excellent catalytic carbonization ability, so that during combustion, it exhibits a faster carbon layer formation speed and stronger self-extinguishing properties when away from the fire.
[0034] 3. The present invention improves the flame retardant properties of the core material by adding linalool, and utilizes the conjugated effect of the substance obtained after high-temperature decomposition of linalool to solve the problem of increased smoke generation caused by the unstable carbon layer generated by the flame retardant catalysis. DETAILED DESCRIPTION
[0035] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following examples and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0036] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments are described as follows:
[0037] The polyethylene is low-density polyethylene and can be purchased from any manufacturer; the polyethylene wax has an average molecular weight of 2000-3000 and can be purchased from any manufacturer; the ethylene-octene copolymer is purchased from Shaanxi Didu Pharmaceutical Chemical Co., Ltd.; and the microcrystalline paraffin is purchased from Shandong Cosmai New Materials Co., Ltd.
[0038] Preparation Example 1
[0039] The preparation steps of flame retardant-A are as follows:
[0040] S1, stirring pentaerythritol and phosphorus oxychloride at a molar ratio of 1:2.9 for 6 hours, purifying, and obtaining reactant 1;
[0041] S2, the reactant 1 obtained in step S1 and 4,4'-dihydroxydiphenyl sulfone were stirred at 80°C for 8h in a molar ratio of 1:1.15, and after the stirring, the reactant was washed with acetonitrile, rotary evaporated, and dried at 60°C to constant weight to obtain a reactant 2;
[0042] S3, 450g of zinc nitrate hexahydrate, 1000g of reactant 2 obtained in step S2 and 20L of anhydrous ethanol were stirred at room temperature for 2h, and then 300g of magnesium nitrate hexahydrate-20L of anhydrous ethanol solution was added and stirred for 1h, followed by adding ammonia water to adjust the pH to 9.7±0.2, stirring for 2h, and then heating to 50°C and stirring for 14h, filtering, washing with ethanol, and drying at 80°C to constant weight to obtain flame retardant-A.
[0043] Preparation Example 2
[0044] The preparation steps of flame retardant-B are as follows:
[0045] The difference between this preparation example and preparation example 1 is that in step S3, zinc nitrate hexahydrate is replaced by an equal amount of ferric nitrate nonahydrate.
[0046] Preparation Example 3
[0047] The preparation steps of flame retardant-C are as follows:
[0048] The difference between this preparation example and preparation example 1 is that the molar ratio of reactant 1 and 4,4'-dihydroxydiphenyl sulfone in step S2 is 1:1.
[0049] Preparation Example 4
[0050] The preparation steps of flame retardant-D are as follows:
[0051] The difference between this preparation example and preparation example 1 is that the molar ratio of reactant 1 to 4,4'-dihydroxydiphenyl sulfone in step S2 is 1:3.
[0052] Example 1
[0053] A flame retardant polymer core material for an aluminum composite panel, comprising the following raw materials by weight: 100 parts of polyethylene, 20 parts of flame retardant-A, 1682 parts of antioxidant, 3 parts of lubricant, 4 parts of ethylene-octene copolymer and 4 parts of dimethicone;
[0054] The lubricant contains 2.3 parts of polyethylene wax and 0.7 parts of microcrystalline wax.
[0055] The method for preparing the flame retardant polymer core material for the aluminum composite plate in this embodiment comprises the following steps: polyethylene, flame retardant-A, antioxidant 168, polyethylene wax, microcrystalline wax, ethylene-octene copolymer and dimethicone are mixed at 85° C. for 15 minutes to obtain the flame retardant polymer core material for the aluminum composite plate.
[0056] Example 2
[0057] A flame retardant polymer core material for an aluminum composite panel, comprising the following raw materials by weight: 95 parts of polyethylene, 15 parts of flame retardant-A, 1681 parts of antioxidant, 2 parts of lubricant, 2 parts of ethylene-octene copolymer and 2 parts of distilled water;
[0058] The lubricant contains 1.6 parts of polyethylene wax and 0.4 parts of microcrystalline wax.
[0059] The method for preparing the flame retardant polymer core material for the aluminum composite plate in this embodiment comprises the following steps: polyethylene, flame retardant-A, antioxidant 168, polyethylene wax, microcrystalline wax, ethylene-octene copolymer and dimethicone are mixed at 80° C. for 20 minutes to obtain the flame retardant polymer core material for the aluminum composite plate.
[0060] Example 3
[0061] A flame retardant polymer core material for an aluminum composite panel, comprising the following raw materials by weight: 105 parts of polyethylene, 25 parts of flame retardant-A, 1684 parts of antioxidant, 4 parts of lubricant, 5 parts of ethylene-octene copolymer and 6 parts of distilled water;
[0062] The lubricant contains 2.9 parts of polyethylene wax and 1.1 parts of microcrystalline wax.
[0063] The method for preparing the flame retardant polymer core material for the aluminum composite plate in this embodiment comprises the following steps: mixing polyethylene, flame retardant-A, antioxidant 168, polyethylene wax, microcrystalline wax, ethylene-octene copolymer and dimethicone at 90° C. for 10 minutes to obtain the flame retardant polymer core material for the aluminum composite plate.
[0064] Example 4
[0065] This embodiment provides a flame retardant polymer core material for aluminum composite panels and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that: the flame retardant-A in the raw material is replaced by an equal amount of flame retardant-B.
[0066] Example 5
[0067] This embodiment provides a flame retardant polymer core material for aluminum composite panels and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that: the flame retardant-A in the raw material is replaced by an equal amount of flame retardant-C.
[0068] Example 6
[0069] This embodiment provides a flame retardant polymer core material for aluminum composite panels and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that: the flame retardant-A in the raw material is replaced by an equal amount of flame retardant-D.
[0070] Example 7
[0071] A flame retardant polymer core material for an aluminum composite panel, comprising the following raw materials by weight: 100 parts of polyethylene, 20 parts of flame retardant-A, 1682 parts of antioxidant, 3 parts of lubricant and 4 parts of ethylene-octene copolymer;
[0072] The lubricant contains 2.9 parts of polyethylene wax and 1.1 parts of microcrystalline wax.
[0073] The method for preparing the flame retardant polymer core material for the aluminum composite plate in this embodiment comprises the following steps: mixing polyethylene, flame retardant-A, antioxidant 168, polyethylene wax, microcrystalline wax and ethylene-octene copolymer at 85° C. for 15 minutes to obtain the flame retardant polymer core material for the aluminum composite plate.
[0074] Performance Testing
[0075] 1. Limiting Oxygen Index Test (LOI)
[0076] The aluminum composite panels provided in each embodiment are made of flame retardant polymer core material into 100×6.5×3.2mm 3 The limiting oxygen index test was carried out on the specimens according to the standard GB / T2406-2015. Each sample was repeated 5 times and the average value was taken.
[0077] 2. Vertical burning test
[0078] The aluminum composite panels provided in each embodiment are made of flame retardant polymer core material into 3.2×13×100 mm 3 The specimens were subjected to vertical burning test in accordance with standard ISO-9773, and the results were graded in the following categories: VTM-0, VTM-1, VTM-2 and not applicable, representing that the flammability of the materials gradually increases.
[0079] The performance test results are shown in Table 1.
[0080] Table 1
[0081]
[0082]
[0083] It can be seen from the data in Table 1 that the polymer core materials of Examples 1-3 have good flame retardant properties; compared with Example 1, Example 4 uses ferric nitrate nonahydrate instead of zinc nitrate hexahydrate in the flame retardant raw material, which affects the catalytic carbonization ability of the metal layer in the flame retardant, resulting in a slight decrease in the flame retardant properties of the core material; compared with Example 1, Examples 5-6 change the amount of 4,4'-dihydroxydiphenyl sulfone used in the preparation process of the flame retardant, which may affect the compatibility between the flame retardant and the polyethylene matrix, resulting in the inability of the oxide after the decomposition of the flame retardant to adhere tightly to the resin matrix, so that the barrier to heat propagation is affected; compared with Example 1, the core material of Example 7 does not contain dimethicone, which results in a decrease in the flame retardancy of the core material.
[0084] The embodiments described above do not impose any form of limitation on the present invention. Although the present invention has been disclosed as a preferred embodiment as above, it is not intended to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still falls within the scope of the technical solution of the present invention.
Claims
1. A flame retardant polymer core material for an aluminum composite panel, characterized in that: The invention comprises the following raw materials by weight: 95-105 parts of polyethylene, 15-25 parts of flame retardant, 1-4 parts of antioxidant, 2-4 parts of lubricant and 2-5 parts of toughening agent; wherein the flame retardant is a layered metal-polymer composition.
2. The flame retardant polymer core material for aluminum composite panels according to claim 1, characterized in that: The preparation steps of the flame retardant are as follows: S1, stirring pentaerythritol and phosphorus oxychloride for 5-7 hours, purifying, and obtaining reactant 1; S2, stirring the reactant 1 obtained in step S1 and 4,4'-dihydroxydiphenyl sulfone at 75-85° C. for 7-9 hours, washing, rotary evaporating and drying after the stirring, to obtain reactant 2; S3, zinc nitrate hexahydrate, reactant 2 obtained in step S2 and anhydrous ethanol are stirred at room temperature for 1-3 hours, and then magnesium nitrate hexahydrate-anhydrous ethanol solution is added and stirred for 1-2 hours, followed by adding ammonia water and stirring for 1-3 hours, and then the temperature is raised to 40-60° C. and stirred for 8-16 hours, filtered, washed and dried to obtain the flame retardant.
3. The flame retardant polymer core material for aluminum composite panels according to claim 2, characterized in that: In step S1, the molar ratio of pentaerythritol to phosphorus oxychloride is 1:(2.4-3.6).
4. The flame retardant polymer core material for aluminum composite panels according to claim 2, characterized in that: In the step S2, the molar ratio of reactant 1 to 4,4'-dihydroxydiphenyl sulfone is 1:(1.05-1.25).
5. The flame retardant polymer core material for aluminum composite panels according to claim 2, characterized in that: In the step S3, the mass ratio of zinc nitrate hexahydrate, reactant 2 and magnesium nitrate hexahydrate is (0.38-0.52):1:(0.23-0.37).
6. The flame retardant polymer core material for aluminum composite panels according to claim 1, characterized in that: The lubricant comprises polyethylene wax and microcrystalline wax.
7. The flame retardant polymer core material for aluminum composite panels according to claim 1, characterized in that: The antioxidant is one or more of a hindered phenol antioxidant, a phosphite antioxidant and a thio antioxidant.
8. The flame retardant polymer core material for aluminum composite panels according to claim 1, characterized in that: The toughening agent is ethylene-octene copolymer or maleic anhydride grafted EVA.
9. The flame retardant polymer core material for aluminum composite panels according to claim 1, characterized in that: The raw material further comprises 2-6 parts by weight of coke.
10. A method for preparing a flame retardant polymer core material for an aluminum composite panel according to any one of claims 1 to 8, characterized in that: The method comprises the following preparation steps: mixing polyethylene, flame retardant, antioxidant, lubricant and toughening agent at 80-90° C. for 10-20 minutes to obtain the flame retardant polymer core material for the aluminum composite plate.
Citation Information
Patent Citations
A halogen-free flame-retardant polyethylene material and its preparation method
CN108912445B