ABS composite material and preparation method thereof

By using flame retardants such as decabromodiphenylethane, chloride polyethylene and molybdenum trioxide in ABS materials, combined with precipitated barium sulfate filling, the flame retardant ABS materials are solved in taking into account both the high oxygen index and toughness of the flame retardant ABS materials. Problem, the preparation of high oxygen index and high toughness materials has been achieved, and is suitable for applications in multiple industries.

CN119060489AActive Publication Date: 2024-12-03CHONGQING ORINKO TECH CO LTD CHINA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411229096.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-03
Estimated Expiration
2044-09-03

AI Technical Summary

Technical Problem

While improving the high oxygen index, existing flame retardant ABS materials usually find it difficult to take into account the toughness and impact performance of the materials, resulting in limited applications in the field of security electrical appliances.

Method used

High bromine content of decabromodiphenylethane, chloride polyethylene and molybdenum trioxide are used as flame retardants and synergistic flame retardants, combined with precipitated barium sulfate as mineral powder filler, combined with lubricant and antioxidant, through The twin screw extrusion mechanism is equipped with high oxygen index and high toughness ABS composite material.

Benefits of technology

On the basis of maintaining good toughness and impact performance, the oxygen index of the material is significantly improved, cost reduction, and the safety performance of the material is improved. It is suitable for household appliances, electrical instruments, construction and security industries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an ABS (Acrylonitrile Butadiene Styrene) composite material and a preparation method thereof, and belongs to the technical field of extruded sheets. The ABS composite material comprises the following raw materials in parts by mass: 59-79 parts of ABS resin, 15-25 parts of a flame retardant, 5 parts of a synergistic flame retardant, 5-15 parts of mineral powder and 1 part of a processing aid. The ABS composite material has the properties of flame retardance, high toughness, high oxygen index and the like, the preparation method is simple and feasible, the processing is easy, and the ABS composite material is very suitable for popularization and application in the fields of household appliances, electrical instruments, the building industry, the traffic industry, the security industry and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of extruded sheets, and in particular relates to an ABS composite material and a preparation method thereof. Background Art

[0002] Styrene-butadiene-acrylonitrile (ABS) resin has the characteristics of rigidity and heat resistance of acrylonitrile, glossiness and processability of polystyrene, and impact resistance of polybutadiene, and is widely used in household appliances, office equipment, instruments and meters, transportation, building materials, daily utensils and packaging materials. However, the limiting oxygen index of ordinary ABS resin is only about 18. According to the requirements of the "Building Design Fire Protection Code", in the field of security electrical appliances, the oxygen index of the emergency light shell needs to be greater than 28, and ABS resin needs to be flame-retardant modified before it can be used. At the same time, the modified high oxygen index flame-retardant ABS is usually limited by toughness and has poor impact resistance.

[0003] In order to effectively improve the high oxygen index of flame retardant ABS materials, the common method is to add different mineral powder fillers to the brominated flame retardant system to increase the oxygen index. However, there is a problem with these methods: flame retardants and mineral powder fillers have an antagonistic effect on the flame retardant effect of the material. In the market, high oxygen index flame retardant ABS is usually subject to the material formula system, and the material toughness is generally low. The common flame retardant ABS materials on the market can only take into account some of the properties of flame retardancy, high toughness, and high oxygen index, and it is difficult to meet the use requirements of such products. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an ABS composite material and a preparation method thereof, which solves the problems in the prior art.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] An ABS composite material comprises the following raw materials in parts by weight:

[0007]

[0008] Furthermore, the flame retardant is at least one of decabromodiphenylethane, brominated triazine and chlorinated polyethylene.

[0009] Furthermore, the synergistic flame retardant is at least one of molybdenum trioxide and antimony trioxide.

[0010] Furthermore, the mineral powder is at least one of precipitated barium sulfate and calcium carbonate.

[0011] Furthermore, the processing aid is a combination of a lubricant and an antioxidant.

[0012] Furthermore, the antioxidant is a hindered phenol antioxidant or a phosphite antioxidant.

[0013] Furthermore, the lubricant is one or more combinations of pentaerythritol stearate, silicone powder, and ethylene bis stearamide.

[0014] A method for preparing the above ABS composite material comprises the following steps:

[0015] S1, putting ABS resin, flame retardant, mineral powder, synergistic flame retardant and processing aid into a high-speed mixer according to the weight proportions to mix and obtain a premix;

[0016] S2, feeding the premix from the main feeding port of the twin-screw extruder for melt extrusion, and then plasticizing, extruding and granulating to obtain a high oxygen index and high toughness ABS composite material.

[0017] Further, the screw aspect ratio of the twin-screw extruder is 48: 1. The conditions for melt extrusion of the twin-screw extruder are: zone 1 temperature 190°C, zone 2 temperature 210°C, zone 3 temperature 215°C, zone 4 temperature 215°C, zone 5 temperature 215°C, zone 6 temperature 215°C, zone 7 temperature 220°C, zone 8 temperature 220°C, zone 9 temperature 220°C, zone 10 temperature 210°C, zone 11 temperature 210°C, main feed rate 350kg / h, screw speed 800rpm.

[0018] The above-mentioned ABS composite material is used in the preparation of electronic appliances and automobile parts.

[0019] Beneficial effects of the present invention:

[0020] 1. The flame retardant of the present invention is decabromodiphenylethane with a high bromine content of about 84%, which can reduce the impact effect and maintain good toughness under the condition of a good high oxygen index.

[0021] 2. The synergistic flame retardant molybdenum trioxide selected in the present invention has the effect of significantly improving the oxygen index compared to conventional antimony trioxide. Chlorinated polyethylene is the preferred synergistic catalyst mainly because chlorinated polyethylene, as a saturated rubber, has excellent resistance to heat oxygen aging, ozone aging, acid and alkali, and chemicals. In the composite material prepared by the present invention, chlorinated polyethylene is added to utilize these characteristics to make the composite flame-retardant ABS material have good toughening performance. In addition, CPE contains chlorine, which makes it have excellent flame retardant properties, and also has the characteristics of burning and dripping prevention, which further improves the safety performance of the material. By cooperating with the synergistic flame retardant of molybdenum trioxide, it can effectively improve the oxygen index of the material at the same time.

[0022] 3. The present invention adopts a screened mineral powder filling, and the mineral powder adopted is precipitated barium sulfate, which is added to the flame-retardant ABS. On the one hand, it can help to improve the test data of the oxygen index; on the other hand, because the barium sulfate has a spherical structure, it can minimize the impact on the impact performance of the flame-retardant ABS; while meeting the high oxygen index and high toughness, the cost is also significantly lower than that of conventional materials.

[0023] 4. The high oxygen index, high toughness and flame retardant ABS material of the present invention has a simple and easy preparation method and is easy to process, and is very suitable for promotion and application in the fields of household appliances, electrical instruments, construction industry, transportation industry, security industry, etc. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] An ABS composite material comprises the following raw materials in parts by weight:

[0026]

[0027] Among them, ABS resin is a high-viscosity ABS resin prepared by a low-solvent emulsion method;

[0028] The flame retardant is at least one of high-bromine content decabromodiphenylethane, brominated triazine and chlorinated polyethylene;

[0029] The synergistic flame retardant is at least one of molybdenum trioxide and antimony trioxide;

[0030] The mineral powder is at least one of precipitated barium sulfate and calcium carbonate;

[0031] The processing aid is a mixture of antioxidants and lubricants;

[0032] The lubricant is selected from at least one of an internal lubricant and an external lubricant. The internal lubricant is selected from ethylene bis stearic acid amides (ethylene bis stearamide EBS, modified ethylene bis stearamide TAF, etc.), and the external lubricant can be selected from stearic acid (barium stearate, calcium stearate, etc.); specifically, the lubricant can be selected from one or more of pentaerythritol stearate, silicone powder, and ethylene bis stearamide.

[0033] The antioxidant is a hindered phenol antioxidant or a phosphite antioxidant, such as antioxidant 1010 or antioxidant 168.

[0034] The preparation process of the ABS composite material is specifically described below through the following examples and comparative examples, wherein the raw materials used in the examples and comparative examples are as follows, and the parts indicated in the examples and comparative examples are all parts by mass;

[0035] ABS resin: low melt index emulsion polymerization ABS, ABS AG10NP, Taiwan Chemical Corporation, melt index is 0.6g / 10min at 200℃ and 5kg, commercially available;

[0036] Flame retardant A: Flame retardant with high bromine content of about 84%, decabromodiphenylethane brand name is SAYTEX4010, from Dead Sea Bromine Company in Israel.

[0037] Flame retardant B: a flame retardant with a bromine content of about 64%, brominated triazine, model FR-245, Shandong Shouguang Co., Ltd., commercially available;

[0038] Flame retardant C: chlorinated polyethylene, model CPE135C, Shouguang Hongchuang Environmental Protection Technology Co., Ltd., commercially available;

[0039] Synergistic flame retardants: antimony trioxide, Sb2O3, Changde Chenzhou Antimony Products Co., Ltd., commercially available; molybdenum trioxide, MoO3, molybdenum trioxide from Xingbang Molybdenum Co., Ltd.

[0040] Mineral powder filler: precipitated barium sulfate, 2000 mesh, Shenzhen Ruixing Radiation Protection Engineering Co., Ltd. Calcium carbonate, CaCO3, 1500, Omiya (USA). Mesh commercially available;

[0041] Antioxidants: antioxidant 1010, antioxidant 168, Lionon, commercially available;

[0042] Lubricant: Pentaerythritol stearate, PETS-AP, Italian hair base, commercially available.

[0043] Example 1

[0044] 79 parts of ABS resin, 15 parts of decabromodiphenylethane, 5 parts of antimony trioxide, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate were put into a high-speed mixer and mixed at 500 rpm for 3 minutes to obtain a premix;

[0045] The premix is ​​fed into the main feeding port of the twin-screw extruder for melting and extrusion, and then plasticized, extruded and granulated to obtain a high oxygen index and high toughness flame retardant ABS composite material;

[0046] The screw aspect ratio of the twin-screw extruder is 48:1, and the melt extrusion conditions of the twin-screw extruder are: zone one temperature 190°C, zone two temperature 210°C, zone three temperature 215°C, zone four temperature 215°C, zone five temperature 215°C, zone six temperature 215°C, zone seven temperature 220°C, zone eight temperature 220°C, zone nine temperature 220°C, zone ten temperature 210°C, zone eleven temperature 210°C, main feed rate 350kg / h, screw speed 800rpm.

[0047] Example 2

[0048] The preparation method is the same as that of Example 1, except for the raw materials. The raw materials in this example are: 79 parts of ABS resin, 15 parts of bromotriazine, 5 parts of antimony trioxide, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate.

[0049] Example 3

[0050] The preparation method is the same as that in Example 1, except for the raw materials, the flame retardant decabromodiphenylethane, and the synergist molybdenum trioxide. The raw materials in this example are: 79 parts of ABS resin, 15 parts of decabromodiphenylethane, 5 parts of molybdenum trioxide, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate.

[0051] Comparative Example 1

[0052] The preparation method is the same as that in Example 1, except that the raw materials are flame retardants decabromodiphenylethane and chlorinated polyethylene; the synergist molybdenum trioxide, and the raw materials in this comparative example are: 69 parts of ABS resin, 15 parts of decabromodiphenylethane, 5 parts of molybdenum trioxide, 5 parts of chlorinated polyethylene, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate.

[0053] Comparative Example 2

[0054] The preparation method is the same as that of Example 1, except that the raw materials are flame retardants, decabromodiphenylethane, chlorinated polyethylene; synergist molybdenum trioxide, mineral powder calcium carbonate. The raw materials in this comparative example are: 69 parts of ABS resin, 15 parts of decabromodiphenylethane, 5 parts of molybdenum trioxide, 5 parts of chlorinated polyethylene, 5 parts of calcium carbonate, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate.

[0055] Comparative Example 3

[0056] The preparation method is the same as that of Example 1, except that the raw materials are flame retardants, decabromodiphenylethane, chlorinated polyethylene; synergist molybdenum trioxide, mineral powder barium sulfate. The raw materials in this comparative example are: 69 parts of ABS resin, 15 parts of decabromodiphenylethane, 5 parts of molybdenum trioxide, 5 parts of chlorinated polyethylene, 5 parts of barium sulfate, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate.

[0057] Comparative Example 4

[0058] The preparation method is the same as that of Example 1, except that the raw materials are flame retardants decabromodiphenylethane and chlorinated polyethylene; synergist molybdenum trioxide and mineral powder barium sulfate. The raw materials in this comparative example are: 64 parts of ABS resin, 15 parts of decabromodiphenylethane, 5 parts of molybdenum trioxide, 5 parts of chlorinated polyethylene, 10 parts of barium sulfate, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate.

[0059] Comparative Example 5

[0060] The preparation method is the same as that of Example 1, except that the raw materials are flame retardants decabromodiphenylethane and chlorinated polyethylene; synergist molybdenum trioxide and mineral powder barium sulfate. The raw materials in this comparative example are: 59 parts of ABS resin, 15 parts of decabromodiphenylethane, 5 parts of molybdenum trioxide, 5 parts of chlorinated polyethylene, 15 parts of barium sulfate, 0.5 parts of antioxidant 1010 and 0.5 parts of pentaerythritol stearate.

[0061] Experimental testing;

[0062] The ABS composite materials prepared in the above Examples 1-3 and Comparative Examples 1-5 were simultaneously prepared with ABS raw materials into standard samples for testing, and the specific steps included the following:

[0063] The flame retardant ABS materials prepared in Examples 1-3 and Comparative Examples 1-5 were dried in an oven at 80°C for 4 hours, and injection molded into national standard notched impact strips, national standard bending strips, and flame retardant 2.0 mm strips. The strips used to test the oxygen index were national standard bending strips.

[0064] The reference standards and methods for the test are as follows:

[0065] Melt index test conditions: GB / T 3682, 220℃ / 10kg;

[0066] Impact strength: GB / T 1843, sample size is 80mm×10mm×4mm;

[0067] Flame retardant: UL-94, strip size 128mm×12.8mm×2.0mm;

[0068] Determination of oxygen index: According to the method provided in GB / T2406.2-2009, pretreatment temperature condition is 25°C, humidity condition is 50% RH, and conditioning is carried out for 88 hours. Ignition method: A-top surface ignition method.

[0069] The test results are shown in Table 1 below;

[0070] Table 1 Test results of Examples 1-8 and Comparative Examples 1-5

[0071]

[0072] According to the data of Examples 1-3, it can be seen that the flame retardants with different bromine contents and different synergists have significant differences in the oxygen index and impact of flame retardant ABS; among them, the decabromodiphenylethane in Example 3 combined with the synergist molybdenum trioxide has the best effect. The high-bromine content decabromodiphenylethane is selected mainly because it can provide as much bromine content as possible while maintaining the impact and flame retardant properties, which is conducive to the test of the oxygen index.

[0073] According to Examples 1, 2, and 3, the data of Comparative Example 1 show that in the bromine-based flame retardant system, the flame retardant chlorinated polyethylene synergist can effectively provide oxygen index test, which is increased from 23 to 27, a year-on-year increase of 17%; the impact is increased from 17.3 to 28.4, a significant increase of nearly 50%. At the same time, the melt index is also enhanced to a certain extent, which is beneficial to the processability of the material. This is mainly because chlorinated polyethylene, as a saturated rubber, has excellent resistance to heat oxygen aging, ozone aging, acid and alkali resistance, and chemical drugs. In the composite material prepared by this patent, chlorinated polyethylene is added to utilize these characteristics to make the composite flame retardant ABS material have good toughening performance. In addition, CPE contains chlorine, which makes it have excellent flame retardant properties, and also has the characteristics of burning and dripping prevention, which further improves the safety performance of the material. By coordinating with the synergistic flame retardant of molybdenum trioxide, the oxygen index of the material can be effectively improved at the same time.

[0074] According to the data of Comparative Examples 1, 2, and 3, the oxygen index of the material can be increased from 27 to 29 by selecting different fillers. The data of Comparative Examples 2 and 3 show that the selected barium sulfate can not only effectively increase the oxygen index of the material, but also keep the impact of the material at about 26, which is about 25% higher than the performance of the calcium carbonate filling system 21. The main reason is that the barium sulfate filling is a spherical structure, which has a relatively small impact on the impact of the material; at the same time, it changes the proportion of different components of the material, reduces the flammability, and thus improves the oxygen index.

[0075] According to the data of Examples 1, 2, 3 and Comparative Examples 1, 2, 3, 4, 5, in the bromine flame retardant system, considering the oxygen index, the comprehensive impact consideration is Example 4, which not only maintains a high toughness impact of 24.3, but also has a high oxygen index of 32. They are significantly higher than conventional flame retardants compounded with antimony, molybdenum and other synergistic flame retardants. In addition, since this system uses a high proportion of 10 parts of barium sulfate filling, the comprehensive cost has a great advantage and the market prospect is broad.

[0076] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0077] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. An ABS composite material, characterized in that: The invention comprises the following raw materials in parts by weight:

2. The ABS composite material according to claim 1, characterized in that: The flame retardant is at least one of decabromodiphenylethane, brominated triazine and chlorinated polyethylene.

3. The ABS composite material according to claim 1, characterized in that: The synergistic flame retardant is at least one of molybdenum trioxide and antimony trioxide.

4. The ABS composite material according to claim 1, characterized in that: The mineral powder is at least one of precipitated barium sulfate and calcium carbonate.

5. The ABS composite material according to claim 1, characterized in that: The processing aid is a combination of a lubricant and an antioxidant.

6. The ABS composite material according to claim 5, characterized in that: The antioxidant is a hindered phenol antioxidant or a phosphite antioxidant.

7. The ABS composite material according to claim 5, characterized in that: The lubricant is one or more combinations of pentaerythritol stearate, silicone powder, and ethylene bis stearamide.

8. A method for preparing the ABS composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, putting ABS resin, flame retardant, mineral powder, synergistic flame retardant and processing aid into a high-speed mixer according to the weight proportions to mix and obtain a premix; S2, feeding the premix from the main feeding port of the twin-screw extruder for melt extrusion, and then plasticizing, extruding and granulating to obtain a high oxygen index and high toughness ABS composite material.

9. A method for preparing an ABS composite material according to claim 8, characterized in that: The screw length-diameter ratio of the twin-screw extruder is 48:

1. The conditions for melt extrusion of the twin-screw extruder are: temperature of zone 1 190°C, temperature of zone 2 210°C, temperature of zone 3 215°C, temperature of zone 4 215°C, temperature of zone 5 215°C, temperature of zone 6 215°C, temperature of zone 7 220°C, temperature of zone 8 220°C, temperature of zone 9 220°C, temperature of zone 10 210°C, temperature of zone 11 210°C, main feed rate 350kg / h, screw speed 800rpm.

10. Use of the ABS composite material according to any one of claims 1 to 7 in the preparation of electronic appliances and automobile parts.

Citation Information

Patent Citations

  • Acrylonitrile-butadiene-styrene (ABS) flame-retardant toughened resin and preparation method thereof

    CN102250443A

  • Environment-friendly ABS flame-retardant master batch and preparation method thereof

    CN103030919A

  • High-oxygen-index, low-smoke and flame-retardant ABS material and preparation method thereof

    CN110982213A

  • Auxiliary agent for improving flame retardant property of polymer coiled material

    CN113956582A

  • High Anti-flammable thermoplastic resin composition

    KR1020090121772A