Polyurethane luminescent material with room-temperature phosphorescence characteristic and preparation method thereof

By dispersing heat to activate delayed fluorescent small molecules in polyurethane materials, the problem of difficulty in achieving phosphorescence at room temperature is solved, low-cost and high-stability polyurethane luminescent materials are realized, and its expansion in the fields of optoelectronic equipment and biomarkers application.

CN119060528APending Publication Date: 2024-12-03HENGYANG AIJIE TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411130782.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

It is difficult for existing organic luminescent materials to achieve phosphorescence at room temperature, and traditional materials rely on precious metal elements, resulting in high cost and insufficient stability, limiting the application of polyurethane materials in the fields of optoelectronic equipment and biomarkers.

Method used

By dispersing organic luminescent small molecule material with thermal activation retardant fluorescence characteristics into the polyurethane material and optimizing specific polymerization reaction conditions, a polyurethane luminescent material with room temperature phosphorescence characteristics is prepared, avoiding the use of precious metals.

Benefits of technology

It has realized low cost, high stability and no by-products, and is suitable for large-area applications and expanded the application range of polyurethane materials in the high-tech field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060528A_ABST
    Figure CN119060528A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of organic light-emitting materials, and discloses a polyurethane material with room-temperature phosphorescence characteristics and a preparation method thereof. The material is obtained by dispersing an organic light-emitting small molecular material compound with a thermally activated delayed fluorescence characteristic into a polyurethane material. The polyurethane luminescent material with the room-temperature phosphorescence characteristic prepared by the invention has the advantages of wide material source, simple preparation method, no need of noble metal materials, low cost, no generation of by-products in the preparation process and environmental friendliness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of organic luminescent materials, and more specifically, to a polyurethane luminescent material with room temperature phosphorescence characteristics and a preparation method thereof. Background Art

[0002] Phosphorescence, especially at room temperature, has long been considered a property of inorganic compounds, such as traditional night-shining pearls. For organic compounds, room temperature phosphorescence was once considered difficult to achieve due to the ease with which excitons localize and rapidly deactivate through non-radiative processes, as well as the challenges of spin-forbidden and non-radiative transitions. In addition, traditional organic phosphorescent materials often rely on complexes containing heavy metal elements such as platinum (Pt) or iridium (Ir), which are not only costly but also lack stability under certain conditions.

[0003] Recently, researchers have broken through this limitation and enhanced the phosphorescence properties of organic molecules by introducing heavy atoms such as halogens into organic molecules, or by changing their chemical structure such as deuteration and introducing aromatic carbonyl groups. These strategies, together with embedding luminescent molecules in polymer matrices, create rigid structures similar to crystal environments, significantly suppressing non-radiative decay processes, thereby achieving room temperature phosphorescence of organic compounds. In the field of polymers, introducing phosphorescent groups into specific polymers has been shown to significantly enhance the phosphorescence effect.

[0004] Polyurethane is a versatile synthetic polymer that is widely used in many industries, including home furnishing, automotive, medical and textile, due to its excellent physical and chemical properties, such as high elasticity, good wear resistance and excellent chemical stability. Despite the wide application of polyurethane, it often lacks optical functions in traditional applications, which limits its further application in high-tech fields such as optoelectronic devices, photosensitive materials and biomarkers.

[0005] In order to combine luminescent materials and polyurethane and expand the application of polyurethane materials, the present invention proposes a new type of polyurethane with room temperature phosphorescence properties and a preparation method thereof, which can effectively disperse the phosphorescent groups evenly in the polyurethane matrix and optimize the luminescent stability and optical properties of the phosphorescent groups through specific polymerization reaction conditions.

[0006] To this end, the inventor has conducted useful explorations and attempts and found a solution to the above-mentioned problem. The solution to be introduced below is produced under this background. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a polyurethane luminescent material with room temperature phosphorescence characteristics and a preparation method thereof in view of the deficiencies and defects of the prior art.

[0008] The technical problem solved by the present invention can be achieved by adopting the following technical solutions:

[0009] A method for preparing a polyurethane luminescent material with room temperature phosphorescence characteristics, characterized in that an organic luminescent small molecule material with thermally activated delayed fluorescence characteristics is dispersed in a polyurethane material to obtain a polyurethane luminescent material with room temperature phosphorescence characteristics, wherein the structure of the organic luminescent small molecule material with thermally activated delayed fluorescence characteristics can be represented by formula (1).

[0010]

[0011] In a preferred embodiment of the present invention, in the polyurethane luminescent material with room temperature phosphorescence characteristics, the organic small molecule material with thermally activated delayed fluorescence characteristics and the polyurethane material are mixed in a mass ratio of 0.1%-5%.

[0012] In a preferred embodiment of the present invention, the polyurethane material comprises a polyurethane material component A and a polyurethane material component B. After the organic small molecule material having thermally activated delayed fluorescence properties is fully mixed with the polyurethane material component A, it is added to the polyurethane material component B, fully stirred, and cured for 6 days to obtain a polyurethane luminescent material having room temperature phosphorescence properties.

[0013] The preparation method of the polyurethane material component B is as follows: add isophorone diisocyanate into a three-necked bottle, raise the temperature to 65 degrees Celsius, slowly drop a mixture of castor oil and acetyl tributyl citrate therein, and after the dropwise addition is completed, react for 8 hours to obtain component B.

[0014] In a preferred embodiment of the present invention, the mass ratio of the polyurethane material component A to the polyurethane material component B is 1:1.

[0015] In a preferred embodiment of the present invention, the polyurethane luminescent material with room temperature phosphorescence characteristics obtained by a method for preparing a polyurethane luminescent material with room temperature phosphorescence characteristics has a phosphorescence lifetime of 0.42s-1.4s.

[0016] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0017] (1) The polyurethane material with room temperature phosphorescence properties prepared by the present invention has a wide range of material sources and a simple preparation method.

[0018] (2) The polyurethane material with room temperature phosphorescence properties prepared by the present invention does not require the use of precious metal materials and has low cost.

[0019] (3) The polyurethane material with room temperature phosphorescence properties prepared by the present invention can be used to prepare large-area materials and has a wide range of application scenarios.

[0020] (4) The polyurethane material with room temperature phosphorescence properties prepared by the present invention has the advantage of being environmentally friendly and has no by-products produced during the preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 It is the mass spectrum of the target product formula (1) in the present invention.

[0023] Figure 2 The hydrogen nuclear magnetic resonance spectrum of the target product of formula (1) in the present invention is shown in FIG.

[0024] Figure 3 The luminescence spectra of the target product (1) of the present invention at different temperatures are shown in FIG.

[0025] Figure 4 The luminescence lifetime of the target product of formula (1) in the present invention at different temperatures.

[0026] Figure 5 This is a phosphorescence spectrum diagram of the polyurethane luminescent material with room temperature phosphorescence characteristics in Examples 1-3 of the present invention.

[0027] Figure 6 This is a phosphorescence lifetime diagram of the polyurethane luminescent material with room temperature phosphorescence characteristics in Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0028] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below.

[0029] The embodiment of the present invention needs to first obtain an intermediate product through chemical synthesis, and then obtain the target product formula (1) through chemical synthesis of the intermediate product. The target product formula (1) is an organic small molecule material with thermally activated delayed fluorescence characteristics, and then the target product (1) is chemically synthesized into a polyurethane luminescent material with room temperature phosphorescence characteristics.

[0030] Example of obtaining intermediate product: In a three-necked reaction bottle containing 1,8-naphthalene dicarboxylic anhydride (3g, 15.14mmol), 100mL of acetic acid was added to dissolve the solid. After nitrogen was filled and kept for 15 minutes, 2-bromoaniline (3.12g, 18.17mmol) was added to the system, and then the temperature of the reaction mixture was raised to 110°C. After the reaction continued for 12 hours under this condition, the mixture was poured into pre-cooled ice water for rapid cooling. Finally, the product was purified by filtration and column chromatography to obtain 4.8g of intermediate product with a yield of 90%. The following is the chemical reaction formula for preparing the intermediate product.

[0031]

[0032] Example of obtaining the target product formula (1): Take the above intermediate product (2g, 5.68mmol) and transfer it to a dry three-necked bottle, and dissolve it with 80mL tetrahydrofuran as a solvent. After standing for 15 minutes under the protection of a nitrogen atmosphere, a small amount of tetrakis triphenylphosphine palladium catalyst (0.05g, 0.043mmol) and potassium carbonate solution are introduced into the system. Subsequently, 3-(9H-carbazole-9-yl)phenylboronic acid (2.45g, 8.52mmol) is added, and the reaction temperature is set at 45°C and continued for 6 hours. After the reaction is completed, dichloromethane is used for three extractions and washed with water three times. After drying with anhydrous sodium sulfate, the product is purified by column chromatography technology to obtain 2.1g of the target product formula (1) with a yield of 72%. The following is the chemical reaction formula for preparing the target product formula (1).

[0033]

[0034] In the embodiment of the present invention, the mass spectrum of the target product (1) measured by mass spectrometer is shown in Figure 1 As shown, the H NMR spectrum of the target product (1) is shown in Figure 2 As shown, the luminescence spectra of the target product (1) at different temperatures are shown in Figure 3 The luminescence lifetime of the target product (1) at different temperatures is shown in Figure 4 As shown. Figure 3 It can be seen that the luminescence intensity of the target product (1) gradually increases with increasing temperature; Figure 4 It can be seen that the luminescent long-life component of the target product formula (1) increases with increasing temperature. The target product formula (1) exhibits the luminescent characteristics of thermally activated delayed fluorescence.

[0035] The final product is a polyurethane luminescent material with room temperature phosphorescence properties. The preparation method is to disperse an organic small molecule material with thermally activated delayed fluorescence properties into a polyurethane material to obtain a polyurethane luminescent material with room temperature phosphorescence properties.

[0036] Among them, in the polyurethane luminescent material with room temperature phosphorescence characteristics, the organic small molecule material with thermally activated delayed fluorescence characteristics, that is, the target product formula (1) and the polyurethane material are mixed in a mass ratio of 0.1%-5%.

[0037] In addition, in the embodiment of the present invention, the polyurethane material includes a polyurethane material component A and a polyurethane material component B. The preparation method of the polyurethane material component A is to mix F524 resin and PTMG-2000 polytetrahydrofuran in a mass ratio of 9 to 2. In the embodiment of the present invention, the F524 resin refers to polyaspartic acid ester resin, which is a solvent-free resin with secondary amino groups that can react with -NCO. PTMG-2000 refers to polytetrahydrofuran, also known as polytetrahydrofuran ether glycol.

[0038] The preparation method of the polyurethane component B is as follows: a predetermined amount of isophorone diisocyanate is added to a three-necked bottle, and then a mixed solution consisting of castor oil and tributyl acetyl citrate is gradually added dropwise at 65° C. After the addition is completed, the reaction is maintained for 8 hours to synthesize a polyurethane prepolymer, i.e., the polyurethane material component B.

[0039] In the embodiment 1 of the present invention for preparing a polyurethane luminescent material having room temperature phosphorescence characteristics, 5 g of polyesteramine material A component is weighed, 0.01 g to 0.02 g of the target product of formula (1) is added, 5 g of polyesteramine material B component is added after sufficient mixing, the mixture is stirred evenly at room temperature, and then cured at room temperature for 6 days to obtain a luminescent polyurethane material. In the embodiment of the present invention, the mass ratio of polyurethane material A component to polyurethane material B component is 1:1.

[0040] The preparation method of Example 2 is the same as that of Example 1, except that the mass of the target product of formula (1) added is 0.1 g.

[0041] The preparation method of Example 3 is the same as that of Example 1, except that the mass of the target product of formula (1) added is 0.2 g.

[0042] Example Example 1 Example 2 Example 3 Add target product formula (1) mass (g) 0.01-0.02 0.1 0.2 Measured maximum phosphorescence emission wavelength (nm) 528 528 528 Phosphorescence lifetime(s) 0.42 1.4 0.91

[0043] Table 1

[0044] See Table 1 and combined Figure 5 , Figure 6 As shown, it can be seen that the obtained polyurethane materials all have obvious phosphorescence phenomenon. Under the fluorescence spectrometer test, the maximum emission wavelength of the phosphorescence is consistent, which is 528nm. The luminescence lifetimes of the phosphorescence are 0.42s, 1.4s, and 0.91s respectively.

[0045] In summary, we have designed a polyurethane material with room temperature phosphorescence, which has high luminescence efficiency, simple and easy-to-obtain raw materials, low synthesis cost, no need for heavy metal materials, few by-products in the entire synthesis process, and can prepare large-area polyurethane phosphorescent materials.

[0046] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a polyurethane luminescent material having room temperature phosphorescence characteristics, characterized in that: An organic light-emitting small molecule material having a thermally activated delayed fluorescence characteristic is dispersed in a polyurethane material to obtain a polyurethane light-emitting material having a room temperature phosphorescence characteristic. The structure of the organic light-emitting small molecule material having a thermally activated delayed fluorescence characteristic can be represented by formula (1).

2. The method for preparing a polyurethane luminescent material having room temperature phosphorescence properties according to claim 1, characterized in that: In the polyurethane luminescent material with room temperature phosphorescence characteristics, the organic small molecule material with thermally activated delayed fluorescence characteristics and the polyurethane are mixed in a mass ratio of 0.1% to 5%.

3. The method for preparing a polyurethane luminescent material having room temperature phosphorescence properties according to claim 1, characterized in that: The polyurethane material comprises a polyurethane material component A and a polyurethane material component B. After the organic small molecule material having a thermally activated delayed fluorescence property is fully mixed with the polyurethane material component A, the organic small molecule material is added to the polyurethane material component B, the mixture is fully stirred, and the polyurethane luminescent material having a room temperature phosphorescence property is obtained after curing for 6 days. The preparation method of the polyurethane material component A is as follows: F524 resin and PTMG-2000 polytetrahydrofuran are mixed in a mass ratio of 9 to 2; The preparation method of the polyurethane material component B is as follows: add isophorone diisocyanate into a three-necked bottle, raise the temperature to 65 degrees Celsius, slowly drip a mixture of castor oil and acetyl tributyl citrate, and after the dripping is completed, react for 8 hours to obtain the polyesteramine material component B.

4. The method for preparing a polyurethane luminescent material having room temperature phosphorescence properties according to claim 3, characterized in that: The mass ratio of the polyurethane material component A to the polyurethane material component B is 1:

1.

5. The polyurethane luminescent material with room temperature phosphorescence characteristics obtained by the preparation method of a polyurethane luminescent material with room temperature phosphorescence characteristics according to any one of claims 1 to 4, wherein the phosphorescence lifetime is 0.42s-1.4s.

Citation Information

Cited By

  • Amino silicon dioxide confinement carbon dot-based waterborne polyurethane with ultra-long phosphorescence service life and preparation method thereof

    CN121609874A