High-temperature-resistant low-shrinkage silicone rubber and preparation thereof

The formulation of polysilazane-modified carbon nanotubes in silicone rubber addresses the issues of poor high temperature resistance and shrinkage, ensuring improved thermal stability and reduced shrinkage through a specialized preparation process.

CN119060545APending Publication Date: 2024-12-03CHUZHOU JUNYUE MACROMOLECULE NEW MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411374224.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing silicone rubber exhibits poor high temperature resistance and significant shrinkage during demolding, posing challenges for precise control of rubber part dimensions and mechanical properties.

Method used

A high temperature resistant and low shrinkage silicone rubber formulation comprising methyl vinyl silicone rubber, hydroxy silicone oil, a di-tetra-vulcanizing agent, and polysilazane-modified carbon nanotubes, with a specific preparation process involving polysilazane and carbon nanotube modification, followed by pressurized heating and vulcanization.

Benefits of technology

The solution provides silicone rubber with enhanced high temperature resistance and reduced shrinkage, maintaining dimensional stability and mechanical integrity under elevated temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005068303010000041
    Figure BDA0005068303010000041
Patent Text Reader

Abstract

The invention discloses high-temperature-resistant low-shrinkage silicone rubber and preparation thereof, and belongs to the technical field of high polymer materials. The high-temperature-resistant low-shrinkage silicone rubber comprises the following raw materials in parts by weight: 100 parts of methyl vinyl silicone rubber, 6 parts of hydroxyl silicone oil, 16-20 parts of an additive and 1-2 parts of a vulcanizing agent, the additive is a polysilazane modified carbon nano tube. The preparation method of the high-temperature-resistant low-shrinkage silicone rubber comprises the following steps: S1, preparing the additive; and S2, weighing the raw materials in parts by weight, uniformly mixing, and pressurizing, heating and vulcanizing in a press vulcanizer. The polysilazane modified carbon nanotube is used as an additive, so that the silicone rubber has good high temperature resistance and low shrinkage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to high-temperature-resistant and low-shrinkage silicone rubber and its preparation. Background Art

[0002] Silicone rubber refers to a rubber whose main chain is composed of alternating silicon atoms and oxygen atoms, and two organic groups are usually connected to the silicon atoms. Ordinary silicone rubber is mainly composed of silicon-oxygen chain segments containing methyl and a small amount of vinyl. It is widely used in the construction industry, electronics industry, molds, automobiles, ships, aviation and other fields, and also plays an important role in the medical field.

[0003] At present, ordinary silicone rubber has a certain high temperature resistance. It can maintain long-term operation at a temperature of 180°C, maintain elasticity for several weeks at a temperature slightly higher than 200°C, and can instantly withstand high temperatures above 300°C. However, with the development of technology, the current high temperature resistance of silicone rubber can no longer meet the requirements of some special fields or special heat-resistant equipment.

[0004] In order to improve the mechanical properties of silicone rubber, it can generally be vulcanized. However, after silicone rubber products are vulcanized and demolded, their geometric dimensions will shrink to varying degrees. The reason for the shrinkage is that during the pressurized and high-temperature vulcanization molding process, the internal linear polymer chains of the rubber raw rubber are three-dimensionally cross-linked into a network, and the internal stress of the rubber increases. In addition, the material itself has the characteristics of thermal expansion and contraction. Therefore, during the demolding and cooling process, the compressive stress brought by the mold is gradually released, and the rubber product shrinks when it is cold. This brings problems and challenges to the precise control of the size of rubber parts. Summary of the invention

[0005] In order to solve the problems of poor high temperature resistance and easy shrinkage of current silicone rubber, the object of the present invention is to provide high temperature resistance and low shrinkage silicone rubber, which has good high temperature resistance and low shrinkage.

[0006] Another object of the present invention is to provide a preparation method for high-temperature-resistant and low-shrinkage silicone rubber, which has a simple process and is suitable for large-scale application.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] High temperature resistance and low shrinkage silicone rubber, characterized by comprising the following raw materials in parts by weight:

[0009] 100 parts of methyl vinyl silicone rubber;

[0010] 6 parts of hydroxy silicone oil;

[0011] 16-20 parts of additives;

[0012] 1-2 parts of vulcanizing agent;

[0013] Furthermore, the additive is polysilazane-modified carbon nanotubes.

[0014] Furthermore, the vulcanizing agent is a di-tetra-vulcanizing agent; the di-tetra-vulcanizing agent has high vulcanization activity, fast decomposition speed, and has the characteristics of achieving a satisfactory crosslinking degree in one vulcanization, without the need for secondary vulcanization, which can save costs.

[0015] Another object of the present invention is achieved by the following technical solution: Preparation of high temperature resistant and low shrinkage silicone rubber comprises the following steps:

[0016] S1. Preparation of additives: adding acyl chloride carbon nanotubes to DMF, ultrasonicating at 50-60° C. for 30-60 min, adding pyridine and polysilazane, stirring at room temperature for 22-24 h, filtering, washing, drying and grinding to obtain polysilazane-modified carbon nanotubes;

[0017] S2. Weigh the raw materials by weight, mix them evenly, and place them in a flat vulcanizing machine for pressurized heating and vulcanization.

[0018] Furthermore, the polysilazane in step S1 is prepared by the following steps: dissolving dimethyldichlorosilane and methyltrichlorosilane in tetrahydrofuran, stirring for 10-15 minutes until the mixture is uniformly mixed, lowering the temperature of the reaction system to -20°C by a liquid nitrogen-ethanol system, introducing ammonia gas to react for 2-3 hours, centrifuging and filtering to obtain a colorless transparent liquid, and removing tetrahydrofuran from the colorless transparent liquid by rotary evaporation at 35-40°C to obtain a colorless transparent liquid polysilazane.

[0019] Furthermore, the volume ratio of dimethyldichlorosilane to methyltrichlorosilane is 4:3;

[0020] The flow rate of the ammonia gas is 30 mL / min; ammonia is a key raw material for introducing nitrogen into synthetic silicon nitrogen rubber. Too small a flow rate may lead to insufficient nitridation. When the ammonia flow rate is too large, it may cause the reaction rate to be too fast, resulting in local overheating or uneven reaction. Therefore, the ammonia flow rate used in the present invention is 30 mL / min.

[0021] Furthermore, the chlorinated carbon nanotubes in step S1 are prepared by the following steps: taking carboxylated multi-walled carbon nanotubes, adding thionyl chloride and DMF thereto, stirring and reacting at 65-70° C. for 22-24 hours, washing and drying to obtain chlorinated carbon nanotubes;

[0022] Furthermore, the usage ratio of the carboxylated multi-walled carbon nanotubes, thionyl chloride and DMF is 0.8 g:80 mL:5 mL.

[0023] Furthermore, the usage ratio of the chlorinated carbon nanotubes, DMF, pyridine and polysilazane in step S1 is 10 g: 100 mL: 0.5 mL: 8-10 g.

[0024] Furthermore, the vulcanization temperature of the vulcanization in step S2 is 150-170° C., the vulcanization pressure is 5-10 MPa, and the vulcanization time is 20-30 min.

[0025] Beneficial effects of the present invention:

[0026] (1) The present invention uses polysilazane-modified carbon nanotubes as additives, which can make silicone rubber have good high temperature resistance and low shrinkage. The reason is that under high temperature conditions, the first thing that happens to silicone rubber is the main chain unbuckling degradation caused by the back biting of the terminal hydroxyl groups of the silicone rubber molecular chain. The silanamine group in the polysilazane can inhibit the back biting effect of the terminal hydroxyl groups of the silicone rubber, thereby effectively inhibiting the main chain unbuckling degradation caused by the terminal hydroxyl groups, so that the silicone rubber has good high temperature resistance; polysilazane can also increase the cross-linking degree of silicone rubber, thereby reducing the shrinkage rate of silicone rubber; the surface of the carbon nanotubes has the function of removing free radicals generated during the degradation process of silicone rubber, thereby inhibiting the chain reaction of silicone rubber degradation and improving the high temperature resistance of silicone rubber; the carbon nanotubes can also act as fillers to increase the filling amount of silicone rubber, thereby reducing the shrinkage rate of silicone rubber.

[0027] (2) The present invention uses carbon nanotubes modified with polysilazane as an additive, and combines polysilazane and carbon nanotubes together chemically. The dispersibility of the carbon nanotubes modified with polysilazane in silicone rubber is significantly improved. The introduction of polysilazane can improve the compatibility between the carbon nanotubes and the silicone rubber matrix, reduce agglomeration, and make the carbon nanotubes more evenly distributed in the silicone rubber, so that the polysilazane and carbon nanotubes can better play the role of improving the high temperature resistance of silicone rubber and reducing the shrinkage rate of silicone rubber. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The amounts of raw materials used in Examples 1 to 6 are shown in Table 1:

[0030] Table 1

[0031]

[0032] The preparation of the high temperature resistant and low shrinkage silicone rubber in Examples 1 to 4 comprises the following steps:

[0033] S1. preparing additives;

[0034] S11, preparation of polysilazane: 160 mL of dimethyldichlorosilane and 120 mL of methyltrichlorosilane were dissolved in tetrahydrofuran, stirred for 12 min, the temperature of the reaction system was lowered to -20°C by a liquid nitrogen-ethanol system, 30 mL / min of ammonia gas was introduced to react for 2.5 h, centrifuged and filtered to obtain a colorless transparent liquid, and tetrahydrofuran in the colorless transparent liquid was removed by rotary evaporation at 40°C to obtain a colorless transparent liquid polysilazane;

[0035] S12, preparing acyl chloride carbon nanotubes: taking 0.8 g of carboxylated multi-walled carbon nanotubes, adding 80 mL of thionyl chloride and 5 mL of DMF thereto, stirring and reacting at 70° C. for 24 h, washing and drying, to obtain acyl chloride carbon nanotubes;

[0036] S13, preparing carbon nanotubes modified with polysilazane: adding 10 g of acyl chloride carbon nanotubes into 100 mL of DMF, ultrasonicating at 60° C. for 30 min, adding 0.5 mL of pyridine and 8 g of polysilazane, stirring at room temperature for 24 h, filtering, washing, drying and grinding to obtain carbon nanotubes modified with polysilazane;

[0037] S2. Weigh the raw materials by weight, mix them evenly, place them in a flat vulcanizer, heat them to 160°C, pressurize them to 8MPa and vulcanize them for 30 minutes.

[0038] Example 5

[0039] The preparation of the high-temperature-resistant and low-shrinkage silicone rubber in this embodiment is different from that in Embodiment 1, the "8 g polysilazane" in step S13 is changed to "9 g polysilazane"; the rest of the preparation process remains the same as that in Embodiment 1.

[0040] Example 6

[0041] The preparation of the high-temperature-resistant and low-shrinkage silicone rubber in this embodiment is different from that in Embodiment 1, the "8 g polysilazane" in step S13 is changed to "10 g polysilazane"; the rest of the preparation process remains the same as that in Embodiment 1.

[0042] Comparative Example 1

[0043] The difference between this comparative example and Example 1 is that carbon nanotubes are used as additives; the other raw materials and preparation process remain the same as those in Example 1.

[0044] Comparative Example 2

[0045] The difference between this comparative example and Example 1 is that carboxylated multi-walled carbon nanotubes are used as additives; the other raw materials and preparation process remain the same as those in Example 1.

[0046] Comparative Example 3

[0047] The difference between this comparative example and Example 1 is that polysilazane is used as an additive; the other raw materials and preparation process remain the same as those in Example 1.

[0048] Comparative Example 4

[0049] The difference between this comparative example and Example 1 is that a 1:1 mixture of polysilazane and carbon nanotubes is used as an additive; the other raw materials and preparation process remain the same as those in Example 1.

[0050] The performance tests were performed on the silicone rubbers prepared in Examples 1 to 6 and Comparative Examples 1 to 4. The thermal decomposition temperature of the silicone rubber was tested using a PerkinElmer TGA 4000 thermogravimetric analyzer to evaluate the high temperature resistance of the silicone rubber. The dimensions of the silicone rubber before and after vulcanization were accurately measured using a vernier caliper to calculate its shrinkage rate. The results are shown in Table 2.

[0051] Table 2

[0052] Test items Thermal decomposition temperature (℃) Shrinkage rate (%) Example 1 462 0.77 Example 2 464 0.72 Example 3 467 0.68 Example 4 469 0.63 Example 5 475 0.49 Example 6 472 0.56 Comparative Example 1 440 1.36 Comparative Example 2 445 1.23 Comparative Example 3 447 1.12 Comparative Example 4 452 0.99

[0053] It can be seen from Table 2 that the silicone rubber prepared in Examples 1 to 6 has good high temperature resistance and low shrinkage; compared with Example 1, Example 2 and Example 3, it can be concluded that increasing the amount of the additive is beneficial to increasing the thermal decomposition temperature of the silicone rubber and reducing the shrinkage of the silicone rubber; compared with Example 3 and Example 4, it can be concluded that increasing the amount of the vulcanizing agent is also beneficial to increasing the thermal decomposition temperature of the silicone rubber and reducing the shrinkage of the silicone rubber, because the vulcanizing agent can make the silicone rubber form a stable cross-linked structure during the vulcanization process, so that the silicone rubber has good thermal stability and a lower shrinkage; compared with Example 4, Example 5 and Example 6, it can be concluded that appropriately increasing the amount of polysilazane can make the additive play a better high temperature resistance and low shrinkage performance. When the polysilazane is excessive, the cross-linking degree of the silicone rubber will be too high, making the silicone rubber too hard, affecting its elasticity and stretchability, and causing the shrinkage of the silicone rubber to increase.

[0054] Compared with Example 1, the thermal decomposition temperature of Comparative Example 1 is lower and the shrinkage rate is increased, indicating that the use of carbon nanotubes alone has a poor effect on improving the high temperature resistance and shrinkage resistance of silicone rubber because carbon nanotubes are easy to agglomerate in silicone rubber.

[0055] Compared with Comparative Example 1, Comparative Example 2 has an increased thermal decomposition temperature and a decreased shrinkage rate. The reason is that the introduction of carboxyl groups on the surface of carbon nanotubes can improve the dispersibility and interfacial interaction of CNTs in silicone rubber and enhance the compatibility of CNTs with the silicone rubber matrix, thereby helping to improve the high temperature resistance of silicone rubber and reduce the shrinkage rate of silicone rubber.

[0056] Compared with Example 1, the thermal decomposition temperature of Comparative Example 3 is lower and the shrinkage rate is increased, indicating that the use of polysilazane alone has a poor effect on improving the heat resistance and shrinkage resistance of silicone rubber.

[0057] Compared with Example 1, Comparative Example 4 has a lower thermal decomposition temperature and an increased shrinkage rate, indicating that the effect of mixing polysilazane and carbon nanotubes by physical method is worse than that of combining polysilazane and carbon nanotubes by chemical method. The reason is that after combining polysilazane and carbon nanotubes by chemical method, the dispersibility of carbon nanotubes modified by polysilazane in silicone rubber is significantly improved. The introduction of polysilazane can improve the compatibility between carbon nanotubes and silicone rubber matrix, reduce agglomeration, and make carbon nanotubes more evenly distributed in silicone rubber, so that polysilazane and carbon nanotubes can better play the role of improving the high temperature resistance of silicone rubber and reducing the shrinkage rate of silicone rubber.

[0058] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0059] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. High temperature resistance and low shrinkage silicone rubber, characterized in that: The invention comprises the following raw materials in parts by weight: 100 parts of methyl vinyl silicone rubber; 6 parts of hydroxy silicone oil; 16-20 parts of additives; 1-2 parts of vulcanizing agent; The additive is carbon nanotube modified by polysilazane.

2. The high temperature resistant and low shrinkage silicone rubber according to claim 1, characterized in that: The vulcanizing agent is a di-tetra-sulfurizing agent.

3. The preparation of the high temperature resistant and low shrinkage silicone rubber according to any one of claims 1 to 2, characterized in that: The steps include: S1. Preparation of additives: adding acyl chloride carbon nanotubes to DMF, ultrasonicating at 50-60° C. for 30-60 min, adding pyridine and polysilazane, stirring at room temperature for 22-24 h, filtering, washing, drying and grinding to obtain polysilazane-modified carbon nanotubes; S2. Weigh the raw materials by weight, mix them evenly, and place them in a flat vulcanizing machine for pressurized heating and vulcanization.

4. The preparation of high temperature resistant and low shrinkage silicone rubber according to claim 3, characterized in that: The polysilazane in step S1 is prepared by the following steps: dissolving dimethyldichlorosilane and methyltrichlorosilane in tetrahydrofuran, stirring for 10-15 minutes, lowering the temperature of the reaction system to -20°C by a liquid nitrogen-ethanol system, introducing ammonia gas to react for 2-3 hours, centrifuging and filtering to obtain a colorless transparent liquid, and removing tetrahydrofuran from the colorless transparent liquid by rotary evaporation at 35-40°C to obtain a colorless transparent liquid polysilazane.

5. The preparation of high temperature resistant and low shrinkage silicone rubber according to claim 4, characterized in that: The volume ratio of dimethyldichlorosilane to methyltrichlorosilane is 4:3; The flow rate of the ammonia gas introduced is 30 mL / min.

6. The preparation of high temperature resistant and low shrinkage silicone rubber according to claim 3, characterized in that: The acyl chloride carbon nanotubes in step S1 are prepared by the following steps: taking carboxylated multi-walled carbon nanotubes, adding thionyl chloride and DMF thereto, stirring and reacting at 65-70° C. for 22-24 hours, washing and drying to obtain acyl chloride carbon nanotubes.

7. The preparation of high temperature resistant and low shrinkage silicone rubber according to claim 6, characterized in that: The usage ratio of the carboxylated multi-walled carbon nanotubes, thionyl chloride and DMF is 0.8-1 g: 80-100 mL: 5 mL.

8. The preparation of high temperature resistant and low shrinkage silicone rubber according to claim 3, characterized in that: The usage ratio of the chlorinated carbon nanotubes, DMF, pyridine and polysilazane in step S1 is 10 g: 100 mL: 0.5 mL: 8-10 g.

9. The preparation of high temperature resistant and low shrinkage silicone rubber according to claim 3, characterized in that: The vulcanization temperature of the vulcanization in step S2 is 150-170° C., the vulcanization pressure is 5-10 MPa, and the vulcanization time is 20-30 min.

Citation Information

Cited By

  • Flexible fireproof cable and preparation method thereof

    CN121086533A