Special fluorinated silicone rubber and preparation process thereof

By adding reinforcement materials and crosslinking agents to fluorosilicone rubber, the degree of crosslinking is improved through high-pressure vulcanization process, the performance decay of fluorosilicone rubber in high temperature and extreme environments is solved, and its mechanical properties and stability are significantly improved. Suitable for high demanding aerospace and automotive fields.

CN119060547APending Publication Date: 2024-12-03ZHEJIANG YUANTONG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411427553.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Existing fluorosilic rubbers have decreased mechanical strength and elasticity in long-term high-temperature environments and lack stability. They are prone to aging, hardening or expanding when used in high-temperature, low-temperature and extreme chemical environments, and have poor processing performance, making it difficult to meet aerospace and automobiles. High requirements in other fields.

Method used

Special fluorosilic rubber with specific ratios and its preparation process include adding reinforcement materials, crosslinking agents and silane coupling agents to the fluorosilic rubber, thereby increasing the crosslinking degree through high-pressure sealing reaction and vulcanization process to form a more stable Silicon-oxygen bonds and boronyl groups enhance the mechanical properties and chemical resistance of the material.

Benefits of technology

It significantly improves the mechanical properties, tensile strength, wear resistance and compression deformation properties of fluorosilic rubber, enhances stability and durability in extreme environments, and is suitable for high-temperature, low-temperature and complex chemical environments, extending its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005082592310000061
    Figure BDA0005082592310000061
  • Figure BDA0005082592310000071
    Figure BDA0005082592310000071
  • Figure BDA0005082592310000081
    Figure BDA0005082592310000081
Patent Text Reader

Abstract

The invention discloses special fluorinated silicone rubber and a preparation process thereof, and relates to the technical field of high polymer materials. The method mainly comprises the following steps: uniformly mixing fluorinated silicone rubber, a reinforcing material and a silane coupling agent according to a ratio; the viscosity of the material is reduced in plastifying equipment, and the fluidity is improved; the cross-linking agent is added under a low-temperature condition to prevent decomposition; vulcanization is carried out under proper temperature and pressure conditions, so that the optimal crosslinking density is ensured; and cooling the vulcanized product and carrying out post-treatment. According to the method, the mechanical property and the compression deformation property of the fluorosilicone rubber are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a special fluorosilicone rubber and a preparation process thereof. Background Art

[0002] Fluorosilicone rubber is a special elastomer that combines the advantages of silicone rubber and fluororubber. Due to its excellent heat resistance, oil resistance, chemical resistance and low-temperature flexibility, it has been widely used in aerospace, automotive industry, petrochemical industry, electronics and electrical fields. Its molecular structure contains both silicon oxygen bonds (Si-O-Si) and fluorine atoms (CF), which makes it have the high temperature stability of silicone rubber and the chemical resistance of fluororubber. This unique structure makes it possible to use fluorosilicone rubber in a variety of extreme environments.

[0003] However, despite the many excellent properties of fluorosilicone rubber, its use under some harsh conditions still has certain limitations. For example, under long-term high temperatures, the heat resistance of fluorosilicone rubber will gradually decrease, resulting in reduced mechanical strength and elasticity. In highly corrosive environments, especially when exposed to some highly active chemicals, traditional fluorosilicone rubber is not stable enough and is prone to aging, hardening, and even cracking, which affects its service life. In addition, the processing performance of fluorosilicone rubber is poor, especially in large-scale industrial production. How to improve the material's fluidity and processing stability is still a difficult problem that needs to be solved.

[0004] Specifically, the aerospace industry places extremely high demands on sealing materials, which must maintain good mechanical properties and sealing properties under high and low temperatures and in complex chemical environments. The performance of existing fluorosilicone rubber under these conditions cannot fully meet the requirements, especially for some applications that require long-term use in ultra-high temperatures (>250°C) or extreme chemical media (such as strong acids, strong alkalis or oxidizing gases). Traditional fluorosilicone rubber is prone to material degradation, aging, expansion and other problems.

[0005] In the automotive industry, engines and their accessories require materials with excellent oil and fuel resistance. Fluorosilicone rubber has also shown certain advantages in such applications. However, when used under high temperature and high pressure conditions, traditional fluorosilicone rubber will harden, resulting in seal failure. In addition, with the development of new energy vehicles, electric vehicles have also put forward new requirements for the high voltage and low temperature resistance of sealing materials, and the current fluorosilicone rubber still has room for improvement in flexibility at extremely low temperatures (such as below -60°C).

[0006] Therefore, although the fluorosilicone rubber in the prior art shows good application prospects in many fields, there is still the problem of performance degradation in long-term high-temperature environments in actual applications. When fluorosilicone rubber is exposed to a high temperature environment above 250°C for a long time, its mechanical strength and elasticity decrease, affecting its service life. Summary of the invention

[0007] The present invention aims to overcome the deficiencies in the prior art and provide a special fluorosilicone rubber and its preparation process with higher stability, durability and processing adaptability under extreme environments, which is particularly suitable for high-demand application fields such as aerospace, automobile manufacturing and national defense and military industry.

[0008] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0009] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0010] By weight, 95-115 parts of fluorosilicone rubber, 5-10 parts of reinforcing material, 1-3 parts of cross-linking agent, and 0.5-2 parts of silane coupling agent.

[0011] In some embodiments of the present invention, the fluorine content in the fluorosilicone rubber is 20%-30%.

[0012] In some embodiments of the present invention, the preparation method of the reinforcing material is:

[0013] S1: Add 0.03-0.2 parts of cerium chloride, 10-15 parts of dicyclopentene methacrylate, 0.5-3 parts of acetic acid and 450-520 parts of DMF by weight into a high-pressure sealed reactor in a reactor 1, heat to 80-90°C and stir to react for 50-100 minutes;

[0014] S2: Add 100-120 parts of fumed silica, 3-6 parts of mercaptosiloxane, and 1000-1200 parts of ethanol to the reaction kettle 2 by weight, stir and react at 40-60°C for 120-180 minutes, filter, and dry to obtain additive A;

[0015] S3: Add 50-60 parts of auxiliary agent A to the reaction kettle 1, then add 0.05-0.5 parts of 1.2-dimercapto-o-carborane and 2-5 parts of triethylamine, heat up, stir to react, then distill to remove DMF, dry, and obtain a reinforcing material.

[0016] In some embodiments of the present invention, the mercaptosiloxane is selected from at least one of γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane.

[0017] In some embodiments of the present invention, the crosslinking agent is selected from one or a combination of dichlorobenzoyl peroxide (DCP), diisopropylbenzene peroxide (DI BP), methyl isobutyryl peroxide (PBO), and bis(tert-butylperoxy)ethylene dicarbonate (BI BP).

[0018] In some embodiments of the present invention, the silane coupling agent is selected from one or a combination of γ-aminopropyltriethoxysilane (APTES), γ-methacryloxypropyltrimethoxysilane (MPS), vinyltrimethoxysilane (VTMS), and γ-glycidoxypropyltrimethoxysilane (GPTMS).

[0019] In some embodiments of the present invention, the production process is as follows:

[0020] The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0021] In some embodiments of the present invention, the mixing temperature in the mixing stage is 10-50° C., and the mixing time is 30-60 minutes.

[0022] In some embodiments of the present invention, the primary vulcanization temperature is 150-170° C., the time is 8-20 min, and the pressure is 10-20 MPa; the secondary vulcanization temperature is 200° C., the time is 4 h, and no pressure is required.

[0023] Brief description of the reaction mechanism:

[0024] 1. Reaction of hydroxy silica with mercaptosiloxane

[0025] The hydroxyl groups (-OH) on the surface of silica can react with siloxane to form modified silica through a silanization reaction, introducing a functional group -SH that can further react.

[0026] 2. Reaction of mercapto white carbon black with acrylate of dicyclopentene cerium:

[0027] -Mercapto (-SH) reacts with the double bond on the acrylate to form a thioether bond structure.

[0028] 3. Reaction of mercaptoborane with propenyl:

[0029] The reaction of mercaptoborane with propenyl can form a stable covalent bond with propenyl through the unique reactivity of borane.

[0030] Technical effect:

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. Enhance mechanical properties:

[0033] The introduced functional groups interact with the molecular chains in the fluororubber matrix to improve the tensile strength and wear resistance of the material.

[0034] 2. Improve rubber compression deformation performance:

[0035] The borane group helps to increase the stability of the material and improves the compression set properties of fluorosilicone rubber.

[0036] 3. Increase chemical resistance:

[0037] Fluororubber itself has good chemical resistance, and the introduction of dicyclopentenyl and borane groups may further enhance this property, making the material more suitable for use in harsh chemical environments. DETAILED DESCRIPTION

[0038] The preferred embodiments of the present invention are described in detail below so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby making a clearer and more definite definition of the protection scope of the present invention.

[0039] Example 1

[0040] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0041] 95g fluorosilicone rubber, 5g reinforcing material, 1g cross-linking agent, 0.5g silane coupling agent.

[0042] The fluorine content in the fluorosilicone rubber is 20%.

[0043] The preparation method of the reinforcing material:

[0044] S1: In reactor 1, add 0.03g cerium chloride, 10g dicyclopentene methacrylate, 0.5g acetic acid and 450g DMF into a high pressure sealed reactor, heat to 80°C and stir to react for 50min;

[0045] S2: Add 100 g of fumed silica, 3 g of mercaptosiloxane, and 1000 g of ethanol into reactor 2, stir and react at 40° C. for 120 min, filter, and dry to obtain additive A;

[0046] S3: Add 50 g of auxiliary agent A to the reaction kettle 1, then add 0.05 g of 1.2-dimercapto-o-carborane and 2 g of triethylamine, heat up, stir to react, then distill to remove DMF, dry, and obtain a reinforcing material.

[0047] The mercaptosiloxane is selected from γ-mercaptopropyltrimethoxysilane.

[0048] The cross-linking agent is selected from dichlorobenzoyl peroxide (DCP).

[0049] The silane coupling agent is selected from γ-aminopropyltriethoxysilane (APTES).

[0050] The production process is as follows:

[0051] The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0052] The mixing temperature in the mixing stage is 10° C. and the mixing time is 60 minutes.

[0053] The primary vulcanization temperature is 150° C., the time is 20 min, and the pressure is 10 MPa; the secondary vulcanization temperature is 200° C., the time is 4 h, and no pressure is required.

[0054] The test results of the fluorosilicone rubber prepared in this example are as follows:

[0055]

[0056]

[0057] Example 2

[0058] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0059] 105g fluorosilicone rubber, 7.5g reinforcement material, 2g cross-linking agent, 1g silane coupling agent.

[0060] The fluorine content in the fluorosilicone rubber is 25%.

[0061] The preparation method of the reinforcing material:

[0062] S1: In reactor 1, 0.08 g of cerium chloride, 12 g of dicyclopentene methacrylate, 1.5 g of acetic acid and 480 g of DMF were added into a high pressure sealed reactor, and the temperature was raised to 85° C. and stirred for reaction for 75 min;

[0063] S2: Add 110 g of fumed silica, 4 g of mercaptosiloxane, and 1100 g of ethanol into reactor 2, stir and react at 50° C. for 140 min, filter, and dry to obtain additive A;

[0064] S3: Add 55 g of auxiliary agent A to the reaction kettle 1, then add 0.2 g of 1.2-dimercapto-o-carborane and 3 g of triethylamine, heat up, stir to react, then distill off DMF, dry, and obtain a reinforcing material.

[0065] The mercaptosiloxane is selected from γ-mercaptopropyltrimethoxysilane.

[0066] The crosslinking agent is selected from dicumyl peroxide (DI BP).

[0067] The silane coupling agent is selected from γ-methacryloxypropyltrimethoxysilane (MPS).

[0068] The production process is as follows:

[0069] The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0070] The mixing temperature in the mixing stage is 25° C., and the mixing time is 50 minutes.

[0071] The primary vulcanization temperature is 160° C., the time is 15 min, and the pressure is 15 MPa; the secondary vulcanization temperature is 200° C., the time is 4 h, and no pressure is required.

[0072] The test results of the fluorosilicone rubber prepared in this example are as follows:

[0073]

[0074] Example 3

[0075] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0076] 105g fluorosilicone rubber, 7.5g reinforcing material, 2g cross-linking agent, 1.5g silane coupling agent.

[0077] The fluorine content in the fluorosilicone rubber is 25%.

[0078] The preparation method of the reinforcing material:

[0079] S1: In reactor 1, 0.15 g of cerium chloride, 14 g of dicyclopentene methacrylate, 2.5 g of acetic acid and 500 g of DMF were added into a high pressure sealed reactor, and the temperature was raised to 85° C. and stirred for reaction for 75 min;

[0080] S2: Add 110 g of fumed silica, 5 g of mercaptosiloxane, and 1100 g of ethanol into reactor 2, stir and react at 50° C. for 160 min, filter, and dry to obtain additive A;

[0081] S3: Add 55 g of auxiliary agent A to the reaction kettle 1, then add 0.4 g of 1.2-dimercapto-o-carborane and 4 g of triethylamine, heat up, stir to react, then distill off DMF, dry, and obtain a reinforcing material.

[0082] The mercaptosiloxane is selected from γ-mercaptopropyltriethoxysilane.

[0083] The cross-linking agent is selected from methyl isobutyryl peroxide (PBO).

[0084] The silane coupling agent is selected from vinyltrimethoxysilane (VTMS).

[0085] The production process is as follows:

[0086] The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0087] The mixing temperature in the mixing stage is 40° C., and the mixing time is 40 minutes.

[0088] The primary vulcanization temperature is 160° C., the time is 12 minutes, and the pressure is 15 MPa; the secondary vulcanization temperature is 200° C., the time is 4 hours, and no pressure is required.

[0089] The test results of the fluorosilicone rubber prepared in this example are as follows:

[0090]

[0091] Example 4

[0092] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0093] 115g fluorosilicone rubber, 10g reinforcement material, 3g cross-linking agent, 2g silane coupling agent.

[0094] The fluorine content in the fluorosilicone rubber is 30%.

[0095] The preparation method of the reinforcing material:

[0096] S1: In reactor 1, 0.2 g cerium chloride, 15 g dicyclopentene methacrylate, 3 g acetic acid and 520 g DMF were added into a high pressure sealed reactor, heated to 90° C. and stirred for reaction for 100 min;

[0097] S2: Add 120 g of fumed silica, 6 g of mercaptosiloxane, and 1200 g of ethanol into reactor 2, stir and react at 60° C. for 180 min, filter, and dry to obtain additive A;

[0098] S3: Add 60 g of auxiliary agent A to the reaction kettle 1, then add 0.5 g of 1.2-dimercapto-o-carborane and 5 g of triethylamine, heat up, stir to react, then distill off DMF, dry, and obtain a reinforcing material.

[0099] The mercaptosiloxane is selected from γ-mercaptopropyltriethoxysilane.

[0100] The crosslinking agent is selected from bis(tert-butylperoxy)ethylene dicarbonate (BI BP).

[0101] The silane coupling agent is selected from γ-glycidoxypropyltrimethoxysilane (GPTMS).

[0102] The production process is as follows:

[0103] The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0104] The mixing temperature in the mixing stage is 50° C. and the mixing time is 30 minutes.

[0105] The primary vulcanization temperature is 170° C., the time is 8 minutes, and the pressure is 20 MPa; the secondary vulcanization temperature is 200° C., the time is 4 hours, and no pressure is required.

[0106] The test results of the fluorosilicone rubber prepared in this example are as follows:

[0107]

[0108]

[0109] Comparative Example 1

[0110] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0111] 95g fluorosilicone rubber, 1g cross-linking agent, 0.5g silane coupling agent.

[0112] The fluorine content in the fluorosilicone rubber is 20%.

[0113] The cross-linking agent is selected from dichlorobenzoyl peroxide (DCP).

[0114] The silane coupling agent is selected from γ-aminopropyltriethoxysilane (APTES).

[0115] The production process is as follows:

[0116] The fluorosilicone rubber is mixed on an open mill, and the silane coupling agent and the cross-linking agent are gradually added according to the ratio and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to make the cross-linking degree reach more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0117] The mixing temperature in the mixing stage is 10° C. and the mixing time is 60 minutes.

[0118] The primary vulcanization temperature is 150° C., the time is 20 min, and the pressure is 10 MPa; the secondary vulcanization temperature is 200° C., the time is 4 h, and no pressure is required.

[0119] The test results of the fluorosilicone rubber prepared in this example are as follows:

[0120]

[0121]

[0122] Comparative Example 2

[0123] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0124] 95g fluorosilicone rubber, 5g reinforcing material, 1g cross-linking agent, 0.5g silane coupling agent.

[0125] The fluorine content in the fluorosilicone rubber is 20%.

[0126] The preparation method of the reinforcing material:

[0127] S1: In reactor 1, add 0.03g cerium chloride, 10g dicyclopentene methacrylate, 0.5g acetic acid and 450g DMF into a high pressure sealed reactor, heat to 80°C and stir to react for 50min;

[0128] S2: Add 100 g of fumed silica and 1000 g of ethanol into reactor 2, heat to 40° C., stir and react for 120 min, filter, and dry to obtain additive A;

[0129] S3: Add 50 g of auxiliary agent A to the reaction kettle 1, then add 0.05 g of 1.2-dimercapto-o-carborane and 2 g of triethylamine, heat up, stir to react, then distill to remove DMF, dry, and obtain a reinforcing material.

[0130] The cross-linking agent is selected from dichlorobenzoyl peroxide (DCP).

[0131] The silane coupling agent is selected from γ-aminopropyltriethoxysilane (APTES).

[0132] The production process is as follows:

[0133] The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0134] The mixing temperature in the mixing stage is 10° C. and the mixing time is 60 minutes.

[0135] The primary vulcanization temperature is 150° C., the time is 20 min, and the pressure is 10 MPa; the secondary vulcanization temperature is 200° C., the time is 4 h, and no pressure is required.

[0136] The test results of the fluorosilicone rubber prepared in this example are as follows:

[0137]

[0138] Comparative Example 3

[0139] A special fluorosilicone rubber and a preparation process thereof, characterized in that: it comprises the following proportions:

[0140] 95g fluorosilicone rubber, 5g reinforcing material, 1g cross-linking agent, 0.5g silane coupling agent.

[0141] The fluorine content in the fluorosilicone rubber is 20%.

[0142] The preparation method of the reinforcing material:

[0143] S1: In reactor 1, add 0.03g cerium chloride, 10g dicyclopentene methacrylate, 0.5g acetic acid and 450g DMF into a high pressure sealed reactor, heat to 80°C and stir to react for 50min;

[0144] S2: Add 100 g of fumed silica, 3 g of mercaptosiloxane, and 1000 g of ethanol into reactor 2, stir and react at 40° C. for 120 min, filter, and dry to obtain additive A;

[0145] S3: 50 g of auxiliary agent A was added to the reaction kettle 1, and then 2 g of triethylamine was added, the temperature was raised, and the mixture was stirred for reaction, and then DMF was removed by distillation, and the mixture was dried to obtain a reinforcing material.

[0146] The mercaptosiloxane is selected from γ-mercaptopropyltrimethoxysilane.

[0147] The cross-linking agent is selected from dichlorobenzoyl peroxide (DCP).

[0148] The silane coupling agent is selected from γ-aminopropyltriethoxysilane (APTES).

[0149] The production process is as follows:

[0150] The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

[0151] The mixing temperature in the mixing stage is 10° C. and the mixing time is 60 minutes.

[0152] The primary vulcanization temperature is 150° C., the time is 20 min, and the pressure is 10 MPa; the secondary vulcanization temperature is 200° C., the time is 4 h, and no pressure is required.

[0153] The test results of the fluorosilicone rubber prepared in this example are as follows:

[0154]

[0155]

[0156] The above implementation scheme and test results effectively improve the mechanical properties and compression deformation properties of fluorosilicone rubber.

[0157] The specific implementation of the present invention is described in detail, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be thought of by a person skilled in the art within the technical scope disclosed by the present invention without creative work should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope defined in the claims.

Claims

1. A special fluorosilicone rubber and its preparation process, Features: Contains the following ratios: By weight, 95-115 parts of fluorosilicone rubber, 5-10 parts of reinforcing material, 1-3 parts of cross-linking agent, and 0.5-2 parts of silane coupling agent.

2. The special fluorosilicone rubber and its preparation process according to claim 1, It is characterized in that The fluorine content in the fluorosilicone rubber is 20%-30%.

3. The special fluorosilicone rubber and its preparation process according to claim 1, It is characterized in that The preparation method of the reinforcing material: S1: Add 0.03-0.2 parts of cerium chloride, 10-15 parts of dicyclopentene methacrylate, 0.5-3 parts of acetic acid, and 450-520 parts of DMF by weight into a high-pressure sealed reactor in a reactor 1, raise the temperature to 80-90°C, stir and react for 50-100 minutes; S2: Add 100-120 parts of fumed silica, 3-6 parts of mercaptosiloxane, and 1000-1200 parts of ethanol to the reaction kettle 2 by weight, stir and react at 40-60°C for 120-180 minutes, filter, and dry to obtain additive A; S3: Add 50-60 parts of auxiliary agent A to the reaction kettle 1, then add 0.05-0.5 parts of 1.2-dimercapto-o-carborane and 2-5 parts of triethylamine, heat up, stir to react, then distill to remove DMF, dry, and obtain a reinforcing material.

4. The special fluorosilicone rubber and its preparation process according to claim 3, It is characterized in that The mercaptosiloxane is selected from at least one of γ-mercaptopropyltrimethoxysilane and γ-mercaptopropyltriethoxysilane.

5. The special fluorosilicone rubber and its preparation process according to claim 1, It is characterized in that The crosslinking agent is selected from one or a combination of dichlorobenzoyl peroxide (DCP), diisopropylbenzene peroxide (DIBP), methyl isobutyryl peroxide (PBO), and bis(tert-butylperoxy)ethylene dicarbonate (BIBP).

6. The special fluorosilicone rubber and its preparation process according to claim 1, It is characterized in that The silane coupling agent is selected from one or a combination of γ-aminopropyltriethoxysilane (APTES), γ-methacryloxypropyltrimethoxysilane (MPS), vinyltrimethoxysilane (VTMS), and γ-glycidyloxypropyltrimethoxysilane (GPTMS).

7. The special fluorosilicone rubber and its preparation process according to claim 1, It is characterized in that The production process is as follows: The fluorosilicone rubber is mixed on an open mill, and reinforcing materials, silane coupling agents and cross-linking agents are gradually added according to the proportions and mixed evenly; a primary vulcanization is carried out under appropriate temperature and pressure conditions to achieve a cross-linking degree of more than 90%, and then a secondary vulcanization is carried out under high temperature and pressure-free conditions to finally achieve the best cross-linking.

8. The special fluorosilicone rubber and its preparation process according to claim 7, It is characterized in that The mixing temperature in the mixing stage is 10-50° C., and the mixing time is 30-60 minutes.

9. The special fluorosilicone rubber and its preparation process according to claim 7, It is characterized in that The primary vulcanization temperature is 150-170° C., the time is 8-20 min, and the pressure is 10-20 MPa; the secondary vulcanization temperature is 200° C., the time is 4 h, and no pressure is required.