Odor-free latex paint with ultralow VOC (volatile organic compound) and SVOC (solid volatile organic compound) emission and preparation method thereof

By using aqueous acrylic emulsion and specific surfactant combination in latex paint, combined with functional additives, combined with raw material screening of the odor clean technology platform, the odor clean problem of latex paint in ultra-low VOC and SVOC emissions is solved, and excellent results are achieved The environmentally friendly performance and user experience meet a number of certification standards.

CN119060593APending Publication Date: 2024-12-03BEIXIN JIABAOLI COATINGS (GUANGDONG) CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411336881.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

It is difficult to achieve odor cleansing effect while pursuing ultra-low VOC. On the basis of ensuring performance, it is difficult to control the emissions of VOC and SVOC at the same time, affecting environmental performance and user experience.

Method used

Use aqueous acrylic emulsion, branched fatty alcohol alkoxylated surfactants and ethoxy compounds to combine functional additives such as dispersants, defoamers, leveling agents, fungicides and anti-mold agents to strictly control VOC and SVOC content and raw material screening and formula adjustment are carried out through Garberli’s odor clean technology platform to ensure the extremely low odor and environmentally friendly performance of the product.

Benefits of technology

It has achieved extremely low VOC and SVOC emissions of latex paint, met the performance requirements of top paint products of "GB/T 9756-2018", and obtained a number of environmental certifications, including the National Inspection Group I+ Odor Certification Gold Grade and Finland M1 Certification etc. to ensure the environmental performance and user experience of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005059069690000101
    Figure BDA0005059069690000101
  • Figure BDA0005059069690000111
    Figure BDA0005059069690000111
Patent Text Reader

Abstract

The invention relates to the technical field of latex paint, and provides odorless latex paint with ultralow VOC (volatile organic compound) and SVOC (solid volatile organic compound) emission and a preparation method of the odorless latex paint. The odorless emulsion paint provided by the invention is prepared from the following components: 30 to 40 percent of water-based acrylic emulsion, 0.6 to 1.0 percent of surfactant, 0.4 to 1.0 percent of hydroxyethyl cellulose, 15 to 30 percent of pigment, 10 to 20 percent of filler, 1.03 to 3.1 percent of functional additive and the balance of water. The latex paint provided by the invention has extremely low odor and ultra-low SVOC and VOC emission level, various properties meet the requirements of top-coat superior products, the physical properties of a coating film are excellent, the applicability is wide, the latex paint conforms to the national environmental protection policy and the environmental protection requirements of market customers, and the prospect is wide. The invention also provides a preparation method of the odorless latex paint, and the preparation method provided by the invention is simple and feasible, and is suitable for large-scale production and application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of latex paints, and in particular to a clean odor latex paint with ultra-low VOC and SVOC emissions and a preparation method thereof. Background Art

[0002] Latex paint is a type of water-based paint made by adding pigments, fillers and various additives to synthetic resin emulsion as the base material, also known as synthetic resin emulsion paint. According to the different production raw materials, latex paint mainly includes polyvinyl acetate latex paint, ethylene propylene latex paint, pure acrylic latex paint and other varieties. Latex paint has many advantages different from traditional wall paint, such as easy to brush, quick drying, water-resistant and scrub-resistant paint film, etc., and is deeply loved by people.

[0003] Volatile organic compounds (VOC) and semi-volatile organic compounds (SVOC) are the main factors that cause physical damage to people in air pollution. With the emergence of environmental protection, green and safe consumer awareness, the majority of consumers are paying more and more attention to environmental protection performance in their consumption choices of home decoration building materials. As the paint that people are most exposed to in daily life, home decoration paint should be at the forefront of the industry in terms of VOC (volatile organic compounds) and SVOC (semi-volatile organic compounds) emission control during use. In recent years, non-toxic, odorless, and organic volatile-free healthy latex paints have become more and more popular. Countries around the world have introduced increasingly stringent restriction standards. my country has also promulgated environmental labeling product certification conditions, which limit the volatile organic compound content of latex paints. Any paint product with a VOC content below 30g / L is called a low-VOC latex paint; and products with a VOC content below the minimum detection limit of the national standard 18582-2020 are zero-VOC or ultra-low-VOC latex paints.

[0004] However, in order to ensure the performance of latex paint, various additives need to be added during the preparation of latex paint, and the additives usually contain VOC or SVOC. For example, film-forming aids and antifreeze agents are usually added to the latex paint formula, and commonly used film-forming aids such as alcohol ester twelve and commonly used antifreeze agents such as ethylene glycol. Without the addition of film-forming aids, there are disadvantages of stickiness of the paint film and poor stain resistance. Without the addition of antifreeze agents, the freeze-thaw stabilizer of the latex paint is poor, and the VOC and SVOC content of the latex paint will increase significantly after adding film-forming aids and antifreeze agents. A Chinese patent application with publication number CN1737066A discloses an environmentally friendly interior wall latex paint, in which redispersible rubber powder is used as a solid film-forming material to obtain a latex paint with a VOC content of less than 5g / L. However, the addition of redispersible rubber powder will reduce the scrub resistance of latex paint. The scrub resistance of latex paint in this patent can only reach more than 200 times, while "GB / T 9756-2018 Synthetic Resin Emulsion Interior Wall Paint" stipulates that the scrub resistance of superior topcoat needs to reach more than 6,000 times.

[0005] In addition, consumers lack the means to control and detect volatile organic compound emissions, and judging by the smell of the environment has become an important means of monitoring for customers. Current latex paints, while pursuing ultra-low VOCs, usually ignore the requirements for odor and cannot achieve a "zero odor" effect.

[0006] In summary, how to achieve ultra-low VOC and SVOC and zero odor effects while ensuring the performance of latex paint is an urgent problem to be solved in this field. Summary of the invention

[0007] In view of this, the present invention provides a clean latex paint with ultra-low VOC and SVOC emissions and a preparation method thereof. The latex paint provided by the present invention has extremely low odor and ultra-low VOC and SVOC emissions, and at the same time, the various performances of the latex paint can meet the requirements of the topcoat superior product in "GB / T 9756-2018 Synthetic Resin Emulsion Interior Wall Paint".

[0008] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0009] A clean latex paint with ultra-low VOC and SVOC emissions, comprising the following components in percentage by weight:

[0010] 30-40% water-based acrylic emulsion, 0.6-1.0% surfactant, 0.4-1.0% hydroxyethyl cellulose, 15-30% pigment, 10-20% filler, 1.03-3.1% functional additive, and the balance water; the functional additive is composed of a dispersant, a defoamer, a leveling agent, a bactericide, a mildew preventer and a pH adjuster;

[0011] The mass percentage of volatile organic matter in the aqueous acrylic emulsion is less than 100ppm, and the mass percentage of semi-volatile organic matter is less than 200ppm; the minimum film-forming temperature of the aqueous acrylic emulsion is less than 5°C; the solid content of the aqueous acrylic emulsion is 49-51%;

[0012] The mass content of volatile organic matter in the surfactant and functional additive is independently lower than 100 ppm, and the mass percentage content of semi-volatile organic matter is independently lower than 1%;

[0013] The surfactant consists of a first surfactant and a second surfactant; the first surfactant is a branched fatty alcohol alkoxylated surfactant, and the second surfactant is an ethoxylated compound.

[0014] Preferably, the mass content of residual monomers in the aqueous acrylic emulsion is less than 200 ppm;

[0015] The mass ratio of the first surfactant to the second surfactant is 1:3-4.

[0016] Preferably, the model of the water-based acrylic emulsion is 7679; the model of the hydroxyethyl cellulose is B30K; the model of the first surfactant is EH-9; and the model of the second surfactant is EF-90.

[0017] Preferably, the dispersant is sodium salt of acrylic acid homopolymer; the defoamer is a mineral oil defoamer; the leveling agent is a polyurethane leveling agent; and the pH adjuster is a sodium hydroxide solution with a mass concentration of 1 to 10%.

[0018] Preferably, the mass percentage of the dispersant in the odorless latex paint with ultra-low VOC and SVOC emissions is 0.3-0.8%, the mass percentage of the defoaming agent is 0.3-0.8%, the mass percentage of the leveling agent is 0.1-0.5%, the mass percentage of the bactericide is 0.2-0.4%, the mass percentage of the mildewcide is 0.1-0.3%, and the mass percentage of the pH adjuster is 0.03-0.3%.

[0019] Preferably, the model of the dispersant is P30; the model of the defoamer is F210; the model of the leveling agent is U300E; the model of the bactericide is MBS 5050 and / or EG CONC; and the model of the mildewcide is PW-40.

[0020] Preferably, the pigment is titanium dioxide; the mesh size of the titanium dioxide is 500 to 1000 mesh;

[0021] The filler is heavy calcium and / or calcined kaolin; the mesh number of the heavy calcium is 600-1500 meshes, and the mesh number of the calcined kaolin is 5000-6000 meshes.

[0022] Preferably, the model of the titanium dioxide is R996, the model of the heavy calcium carbonate is JF-1250, and the model of the calcined kaolin is 80L.

[0023] The present invention also provides a method for preparing the odorless latex paint with ultra-low VOC and SVOC emissions described in the above scheme, comprising the following steps:

[0024] Premixing water, a dispersant, a first surfactant, a defoamer, hydroxyethyl cellulose and a pH regulator to obtain a premix;

[0025] Dispersing the premix, pigment and filler to obtain a dispersed slurry;

[0026] The dispersed slurry is mixed with a water-based acrylic emulsion, a leveling agent, a second surfactant, a mildew preventive, and a bactericide to obtain the odorless latex paint with ultra-low VOC and SVOC emissions.

[0027] Preferably, the stirring speed of the premixing is 300 to 500 rpm; the stirring speed of the dispersing is 700 to 800 rpm; and the stirring speed of the mixing is 500 to 700 rpm.

[0028] The invention provides a clean latex paint with ultra-low VOC and SVOC emissions, comprising the following components in percentage by weight: 30-40% of waterborne acrylic emulsion, 0.6-1.0% of surfactant, 0.4-1.0% of hydroxyethyl cellulose, 15-30% of pigment, 10-20% of filler, 1.03-3.1% of functional additive, and the balance of water; the mass percentage of volatile organic matter in the waterborne acrylic emulsion is less than 100ppm, and the mass content of semi-volatile organic matter is less than 200ppm; the minimum film-forming temperature of the waterborne acrylic emulsion is less than 5°C; the solid content of the waterborne acrylic emulsion is 49-51%; the mass content of volatile organic matter in the surfactant and the functional additive is independently less than 100ppm, and the mass percentage of semi-volatile organic matter is independently less than 1%; the surfactant consists of a first surfactant and a second surfactant; the first surfactant is a branched fatty alcohol alkoxylated surfactant, and the second surfactant is an ethoxylated compound. The present invention strictly controls the VOC and SVOC contents of the water-based acrylic emulsion, the surfactant and the functional additive, and strictly controls the odor and harmful substances brought in by the raw materials, so as to ensure that the requirements of the top environmental protection certification can be met from the raw materials, so that the product does not contain substances that are harmful to the human body, carcinogenic or cause reproductive toxicity, and ensures that the product performs well in environmental protection performance testing and user experience; and, the present invention selects a water-based acrylic emulsion with a minimum film-forming temperature of less than 5°C, which can meet the film-forming temperature requirements in the application of water-based construction coating systems, and there is no need to add film-forming aids containing VOCs and SVOCs to assist in film formation; at the same time, the present invention selects ethoxylated compounds in combination with branched fatty alcohol alkoxylated surfactants, which can ensure the wetting and color-adjusting properties of the product while assisting the emulsion to remain stable in the freeze-thaw cycle test of the coating system, thereby avoiding the addition of antifreeze containing VOCs and SVOCs.

[0029] Furthermore, in terms of odor, the present invention uses Carpoly's odor-free technology platform and a dedicated odor identification team to screen raw materials and develop and adjust the overall formula based on comprehensive environmental indicators, and ultimately determines the model of each raw material. The resulting latex paint product has the industry's top odor-free level.

[0030] The results of the embodiments show that the state, construction performance, low-temperature stability, low-temperature film-forming property, drying time, film appearance, contrast ratio, alkali resistance and scrub resistance of the latex paint provided by the present invention all meet the standards of superior topcoat in "GB / T9756-2018 Synthetic Resin Emulsion Interior Wall Paint", and the scrub resistance reaches 20,000 times; the odor of the latex paint was evaluated with reference to the odor evaluation method in Appendix J of "GB 36246-2018 Synthetic Material Surface Sports Fields for Primary and Secondary Schools", and the score reached 8.9 to 9.5 points (out of 10 points); based on the method in "GB 18582-2020 Limits of Hazardous Substances in Wall Coatings for Buildings", the latex paint of the present invention was tested, and VOC, SVOC, benzene series, formaldehyde, heavy metals, APEO (alkylphenol polyoxyethylene ether compounds), etc. were not detected. On the whole, the final environmental performance of the latex paint provided by the present invention complies with the requirements of GB 18582-2020 "Limits of Hazardous Substances in Interior Decoration and Renovation Materials and Interior Wall Paints"; complies with the U.S. GREENGUARD GOLD Certification gold certification; complies with the U.S. Green Guard (UL) requirements; complies with the Finnish M1 certification requirements; complies with the FDA testing index requirements of the U.S. Food and Drug Administration; complies with the French A+ certification requirements; complies with the requirements of the EU RECH regulations; and meets the National Inspection Group I+ odor certification gold requirements.

[0031] In summary, the latex paint provided by the present invention has extremely low odor and ultra-low SVOC and VOC emission levels during use on the wall, and the coating film has excellent physical properties, is suitable for various construction processes such as brushing, roller coating, and spraying, has a wide range of applicability, is suitable for renovation of old houses, construction of new houses, and various construction environments with rapid occupancy requirements, can meet the country's environmental protection policies and the environmental protection needs of market customers, and has broad market prospects.

[0032] The present invention also provides a method for preparing the odorless latex paint with ultra-low VOC and SVOC emissions described in the above scheme. The preparation method provided by the present invention is simple and easy to implement, and is suitable for large-scale production and application. DETAILED DESCRIPTION

[0033] The present invention provides a clean latex paint with ultra-low VOC and SVOC emissions, comprising the following components in percentage by mass:

[0034] 30-40% water-based acrylic emulsion, 0.6-1.0% surfactant, 0.4-1.0% hydroxyethyl cellulose, 15-30% pigment, 10-20% filler, 1.03-3.1% functional additive, and the balance water; the functional additive is composed of a dispersant, a defoamer, a leveling agent, a bactericide, a mildew preventer and a pH adjuster;

[0035] The mass percentage of volatile organic matter in the aqueous acrylic emulsion is less than 100ppm, and the mass percentage of semi-volatile organic matter is less than 200ppm; the minimum film-forming temperature of the aqueous acrylic emulsion is less than 5°C; the solid content of the aqueous acrylic emulsion is 49-51%;

[0036] The mass content of volatile organic matter in the surfactant and functional additive is independently lower than 100 ppm, and the mass percentage content of semi-volatile organic matter is independently lower than 1%;

[0037] The surfactant consists of a first surfactant and a second surfactant; the first surfactant is a branched fatty alcohol alkoxylated surfactant, and the second surfactant is an ethoxylated compound.

[0038] Unless otherwise specified, the raw materials / components used in the present invention are commercially available.

[0039] In terms of mass percentage, the odorless latex paint with ultra-low VOC and SVOC emissions provided by the present invention includes 30-40% of water-based acrylic emulsion, preferably 32-40%; the mass percentage of volatile organic matter in the water-based acrylic emulsion is less than 100ppm, and the mass percentage of semi-volatile organic matter is less than 200ppm; the minimum film-forming temperature of the water-based acrylic emulsion is less than 5°C; the solid content of the water-based acrylic emulsion is 49-51%; the mass percentage of residual monomers in the water-based acrylic emulsion is preferably less than 200ppm. In a specific embodiment of the present invention, the model of the water-based acrylic emulsion is preferably PLUS 7679, manufactured by BASF. The present invention strictly controls the residual monomer content and the content of VOC and SVOC of the emulsion, so that the emulsion raw material is almost tasteless; and the minimum film-forming temperature of the emulsion used in the present invention is less than 5°C, which meets the film-forming temperature requirements in the application of water-based construction coating systems, and there is no need to add additional film-forming aids containing VOC and SVOC to assist film formation.

[0040] In terms of mass percentage, the odorless latex paint with ultra-low VOC and SVOC emissions provided by the present invention includes 0.6-1.0% surfactant, preferably 0.8-1.0; the surfactant is composed of a first surfactant and a second surfactant; the first surfactant is a branched fatty alcohol alkoxylated surfactant, and the second surfactant is an ethoxylated compound; the mass ratio of the first surfactant to the second surfactant is preferably 1:3-4. In a specific embodiment of the present invention, the model of the first surfactant is preferably EH-9, and the manufacturer is Dow Chemical Co., Ltd.; the model of the second surfactant is preferably EF-90, and the manufacturer is Nouryon Chemical Co., Ltd. The present invention uses the first surfactant and the second surfactant in combination, which can ensure the wetting and color matching properties of the product while helping the emulsion to remain stable in the freeze-thaw cycle test of the coating system.

[0041] The ultra-low VOC and SVOC emission clean latex paint provided by the present invention comprises 0.4-1.0%, preferably 0.5-0.6%, of hydroxyethyl cellulose in terms of mass percentage. In the present invention, the hydroxyethyl cellulose is preferably of the type B30K, and the manufacturer is Lotte Corporation of South Korea; the hydroxyethyl cellulose plays the role of thickening and water retention, which is beneficial to improving the storage stability of the latex paint system, improving the workability, and improving the flatness of the coating film.

[0042] The ultra-low VOC and SVOC emission clean latex paint provided by the present invention comprises 15-30% of pigment, preferably 20-25% by mass percentage. In the present invention, the pigment is preferably titanium dioxide; the mesh number of the titanium dioxide is preferably 500-1000 mesh; in a specific embodiment of the present invention, the model of the titanium dioxide is preferably R996, and the manufacturer is Longman Billions.

[0043] In terms of mass percentage, the odorless latex paint with ultra-low VOC and SVOC emissions provided by the present invention includes 10-20% filler, preferably 10-15%, and more preferably 10-13.5%. In the present invention, the filler is preferably heavy calcium and / or calcined kaolin; when the filler includes heavy calcium and calcined kaolin at the same time, the mass ratio of the heavy calcium and calcined kaolin is preferably 2-5:1; the mesh number of the heavy calcium is preferably 600-1500 mesh, and the mesh number of the calcined kaolin is preferably 5000-6000 mesh. In a specific embodiment of the present invention, the model of the heavy calcium is preferably JF-1250, and the manufacturer is Jiaoling Jinpeng Fine Chemical Co., Ltd.; the model of the calcined kaolin is preferably 80L, and the manufacturer is Tangshan Madison Kaolin Co., Ltd.

[0044] The odorless latex paint with ultra-low VOC and SVOC emissions provided by the present invention comprises 1.03-3.1% of functional additives, preferably 2-3%, in terms of mass percentage; the functional additives are composed of a dispersant, a defoamer, a leveling agent, a bactericide, a mildewicide and a pH adjuster; the dispersant is preferably a sodium salt of an acrylic acid homopolymer; the defoamer is preferably a mineral oil defoamer; the leveling agent is preferably a polyurethane leveling agent; and the pH adjuster is preferably a sodium hydroxide solution with a mass concentration of 1-10%. Specifically, the mass percentage of the dispersant in the odorless latex paint with ultra-low VOC and SVOC emissions is preferably 0.3-0.8%, more preferably 0.5-0.6%, the mass percentage of the defoamer is preferably 0.3-0.8%, more preferably 0.45-0.55%, the mass percentage of the leveling agent is preferably 0.1-0.5%, more preferably 0.25-0.3%, the mass percentage of the bactericide is preferably 0.2-0.4%, more preferably 0.25-0.3%, the mass percentage of the mildewcide is preferably 0.1-0.3%, more preferably 0.2-0.25%, and the mass percentage of the pH regulator is preferably 0.03-0.3%, more preferably 0.05-0.1%. In a specific embodiment of the present invention, the dispersant is preferably of type P30, manufactured by Arkema; ​​the defoamer is preferably of type F210, manufactured by Shanghai Guben Industrial Co., Ltd.; the leveling agent is preferably of type U300E, manufactured by Wanhua Chemical Co., Ltd.; the fungicide is preferably of type MBS 5050 (referred to as the first fungicide) and / or EG CONC (referred to as the second fungicide), wherein both MBS 5050 and EG CONC are manufactured by THOR; in a specific embodiment of the present invention, the first fungicide and the second fungicide are preferably used in combination, and the mass ratio of the first fungicide to the second fungicide is preferably 1:1-2, more preferably 1:1.5; the mildewcide is preferably of type PW-40, manufactured by Troy; the fungicide and mildewcide used in the present invention do not contain formaldehyde, and can avoid odors and harmful substances brought in by the auxiliary agent.

[0045] In the present invention, the pH value of the odorless latex paint with ultra-low VOC and SVOC emissions is preferably 7-9.

[0046] The water-based acrylic emulsion, surfactant and functional additive used in the present invention are all products that have been treated with chemical treatment and steam extraction, and the content of harmful substances such as residual monomers, VOC, formaldehyde, heavy metals, APEO, etc. in the raw materials is strictly controlled to ensure that the requirements of top environmental protection certification can be met from the raw materials, so that the products do not contain substances that are harmful to the human body, carcinogenic or cause reproductive toxicity. For example: select surfactants, pH adjusters, and dispersants that do not contain VOC and have low odor, use fungicides and mildew inhibitors that do not contain formaldehyde, strictly control the odor and harmful substances brought in by the raw materials, and ensure that the product performs well in environmental performance testing and user experience.

[0047] The present invention also provides a method for preparing the odorless latex paint with ultra-low VOC and SVOC emissions described in the above scheme, comprising the following steps:

[0048] Premixing water, a dispersant, a first surfactant, a defoamer, hydroxyethyl cellulose and a pH regulator to obtain a premix;

[0049] Dispersing the premix, pigment and filler to obtain a dispersed slurry;

[0050] The dispersed slurry is mixed with a water-based acrylic emulsion, a leveling agent, a second surfactant, a mildew preventive, and a bactericide to obtain the odorless latex paint with ultra-low VOC and SVOC emissions.

[0051] In the present invention, water, a dispersant, a first surfactant, a defoamer, hydroxyethyl cellulose and a pH regulator are premixed to obtain a premix. In the present invention, the stirring speed of the premix is ​​preferably 300 to 500 rpm, more preferably 350 to 450 rpm; in the present invention, the dispersant, the first surfactant and the defoamer are preferably added to the water in sequence, and then stirring is started, and then the hydroxyethyl cellulose and the pH regulator are slowly added, and stirring is continued for 5 minutes after the addition is completed.

[0052] After obtaining the premix, the present invention disperses the premix, pigment and filler to obtain a dispersed slurry. In the present invention, it is preferred to add pigments and fillers in order from light to heavy and from large oil absorption to small oil absorption; in a specific embodiment of the present invention, when the pigment is titanium dioxide and the filler is heavy calcium and calcined kaolin, the order of addition is titanium dioxide, calcined kaolin, and heavy calcium; the stirring speed of the dispersion is preferably 700-800rpm; the dispersion time is based on the fineness of the dispersed slurry <50μm; in a specific embodiment of the present invention, it is preferred to continue stirring for 15-20min after the pigment and filler are added, and then the slurry is subjected to a scraper fineness test. If the fineness is unqualified, the dispersion time is continued to be extended until the slurry fineness meets the standard.

[0053] After obtaining the dispersed slurry, the present invention preferably mixes the dispersed slurry with a water-based acrylic emulsion, a leveling agent, a second surfactant, a mildew preventer, and a bactericide to obtain the odorless latex paint with ultra-low VOC and SVOC emissions. In the present invention, the mixing speed is preferably 500-700rpm; the mixing includes a first mixing and a second mixing performed in sequence, and the first mixing is preferably: first adding the water-based acrylic emulsion, the leveling agent, and the second surfactant to the dispersed material for stirring and mixing; the first mixing time is preferably 10-15min; the second mixing is preferably: adding a bactericide and a mildew preventer to the mixture obtained by the first mixing in sequence for stirring and mixing; the second mixing time is preferably 8-10min. In a specific embodiment of the present invention, the first mixing is the paint mixing stage, and the second mixing is the terminal mixing stage.

[0054] After the second mixing is completed, the present invention preferably tests the performance indicators of the obtained latex paint, and can filter and package it after passing the test; the performance indicators of the latex paint preferably include: fineness <50μm, specific gravity of 1.40±0.02g / mL, hiding power ≥0.95, Stormer viscosity of 112±4KU, and gloss (60°) of: 3~5GU.

[0055] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] Example 1

[0057] The mass percentages of the components of the odorless latex paint with ultra-low VOC and SVOC emissions prepared in this embodiment are as follows: 32% water-based acrylic emulsion, 0.2% first surfactant, 0.6% second surfactant, 0.5% dispersant, 0.45% defoamer, 0.6% hydroxyethyl cellulose, 20% pigment, 2.5% calcined kaolin, 11% heavy calcium, 0.25% polyurethane leveling agent, 0.1% first bactericide, 0.15% second bactericide, 0.2% mildewcide, 0.05% pH adjuster, and 31.4% water.

[0058] Among them, the water-based acrylic emulsion is produced by BASF. PLUS 7679 water-based acrylic emulsion; the first surfactant is a branched fatty alcohol alkoxylated surfactant of model EH-9 produced by Dow Chemical Company, and the second surfactant is an ethoxylated compound of model EF-90 produced by Nouryon; the dispersant is a sodium salt of acrylic acid homopolymer of model P30 produced by Arkema; ​​the defoamer is a mineral oil defoamer of model F210 produced by Solid Company; the hydroxyethyl cellulose is B30K produced by Lotte Company of South Korea; the pigment is R996 titanium dioxide produced by LOMON Company, the heavy calcium is JF-1250 heavy calcium produced by Jiaoling Jinpeng Company, and the calcined kaolin is 80L calcined kaolin produced by Madison Company; the polyurethane leveling agent is U300E produced by Wanhua Company; the first fungicide is MBS 5050 produced by Sol Company, and the second fungicide is EG CONC produced by Sol Company; the mildew inhibitor is a mildew inhibitor of model PW-40 produced by Troy Company; the pH adjuster is a 10wt% sodium hydroxide aqueous solution.

[0059] The preparation method of latex paint is as follows:

[0060] (1) Premixing: Add dispersant, first surfactant, and defoamer to water in sequence, start the disperser and stir at a low speed (400 rpm), then slowly add hydroxyethyl cellulose and pH adjuster in sequence, and mix and stir for 5 minutes;

[0061] (2) Dispersion of pigments and fillers: titanium dioxide, calcined kaolin and heavy calcium are added to the mixed solution in sequence. After dispersion at high speed (800 rpm) for 15 minutes, the slurry is sent for scraper fineness test. The fineness requirement is <50 μm. After the fineness is qualified, production can continue;

[0062] (3) Paint mixing: slowly add emulsion, polyurethane leveling agent, and second surfactant, and mix at medium speed (600 rpm) for 10 min;

[0063] (4) Terminal mixing: Finally, add the first fungicide, the second fungicide, and the mildew preventer in sequence and mix at medium speed (600 rpm) for 10 minutes.

[0064] (5) Finished product inspection and packaging: Test the product performance indicators (fineness <50μm, specific gravity 1.40±0.02g / mL, hiding power ≥0.95, Stormer viscosity 112±4KU, gloss (60°): 3~5GU), and filter and package after passing the test.

[0065] Example 2

[0066] The raw material model and preparation method are the same as those in the embodiment, and only the mass percentage of each component in the latex paint is adjusted to: emulsion 40%, first surfactant 0.2%, second surfactant 0.8%, dispersant 0.5%, defoamer 0.55%, hydroxyethyl cellulose 0.5%, pigment 25%, calcined kaolin 3%, heavy calcium 7%, polyurethane leveling agent 0.25%, first bactericide 0.1%, second bactericide 0.15%, mildewicide 0.2%, pH adjuster 0.05%, water 21.7%.

[0067] Comparative Example 1

[0068] The other raw materials are the same as those in Example 1, with the only difference being that conventional interior wall styrene-acrylic emulsion is used instead of water-based acrylic emulsion, 1.5% of the water in the formula is replaced by an equal amount of film-forming aid to ensure film formation of the paint, and 1% of the water in the formula is replaced by an equal amount of antifreeze to ensure freeze-thaw stability of the paint; wherein the styrene-acrylic emulsion is a styrene-acrylic emulsion of model 313 produced by Badful Company; the film-forming aid is an alcohol ester twelve film-forming aid produced by Runtai Company; and the antifreeze is ethylene glycol produced by BASF.

[0069] The preparation method of latex paint is similar to that of Example 1, except that the film-forming aid and antifreeze agent are added in step (4), and the other conditions are the same as those of Example 1.

[0070] Comparative Example 2

[0071] The other raw materials were the same as those in Example 1, except that the second surfactant was replaced by polyethylene glycol; the polyethylene glycol was produced by Clariant and its model number was PEG300.

[0072] Comparative Example 3

[0073] The other raw materials were the same as those in Example 1, except that the second surfactant was replaced by an equal amount of water.

[0074] Performance Testing

[0075] The basic performance of the latex paint prepared in Examples 1 to 2 and Comparative Examples 1 to 3 was tested according to the method in GB / T 9756-2018 Synthetic Resin Emulsion Interior Wall Paint to determine whether it meets the requirements of topcoat quality; the basic performance test includes: state in the container, workability, low temperature stability (3 cycles), low temperature film formation, drying time, film appearance, contrast ratio, alkali resistance, and scrub resistance. The test results are shown in Table 1.

[0076] According to the odor evaluation method in Appendix J of GB 36246-2018 Synthetic Surface Sports Grounds for Primary and Secondary Schools, the latex paints prepared in Examples 1 to 2 and Comparative Examples 1 to 3 were evaluated for odor, and the odor was scored on a 10-point scale, with the higher the score, the better the performance. The test results are shown in Table 1.

[0077] According to the method in "GB 18582-2020 Limits of Hazardous Substances in Architectural Wall Coatings", the semi-volatile organic compounds (SVOC), volatile organic compounds (VOC), benzene series (total amount of benzene, toluene, xylene and ethylbenzene), formaldehyde, heavy metals (lead, cadmium, chromium, mercury), and APEO of the latex paints prepared in Examples 1 to 2 and Comparative Examples 1 to 3 were tested. The test results are shown in Table 1.

[0078] Table 1 Performance test results

[0079]

[0080]

[0081] According to the data in Table 1, it can be seen that the performance of the latex paints prepared in Examples 1 to 2 meets the requirements of the superior topcoat in GB / T9756-2018, and has excellent film-forming performance, freeze-thaw cycle resistance and scrub resistance. The scrub resistance of Example 2 reaches 20,000 times, which is much higher than the national standard requirements; and the latex paints prepared in Examples 1 to 2 have high odor scores, and VOC, SVOC, benzene, formaldehyde, heavy metals and APEO are not detected; in Comparative Example 1, conventional interior wall styrene acrylic emulsion is used instead of water-based acrylic emulsion, and film-forming aids and antifreeze agents are added to ensure performance. Although the performance in all aspects meets the requirements of the topcoat of GB / T9756-2018, the odor score is low, and the VOC and SVOC content are high; in Comparative Example 2, the second surfactant is replaced with polyethylene glycol. Although the performance in all aspects meets the requirements of the topcoat of GB / T9756-2018, the SVOC content is high; in Comparative Example 3, the second surfactant is omitted, and the low-temperature stability of the obtained latex paint does not meet the requirements and cannot meet the standards of the topcoat of GB / T 9756-2018. In summary, the present invention can achieve extremely low odor and ultra-low VOC and SVOC emissions on the basis of ensuring that the performance in all aspects meets the standards of the topcoat, through the selection of raw materials and the control of the latex paint formula, and has excellent environmental protection performance and the industry's top odor-free level.

[0082] It can be seen from the above embodiments that the beneficial effects of the present invention are:

[0083] (1) The latex paint of the present invention has excellent environmental performance and has passed the high-end environmental certifications of 7 countries or regions, including the I+ Odor Certification Gold Level of the National Inspection Group, M1 of Finland, A+ of France, Reach of the European Union, UL of the United States, and FDA of the United States. Its environmental protection level and odor-free performance during construction are excellent among similar products on the market. In addition, during use, whether during construction, after construction, or in the long-term process after the wall is actually dry, there will be no strong, irritating odor or volatilization of harmful substances, which effectively guarantees the user experience.

[0084] (2) It will promote the common development of domestic peers, upstream supporting enterprises and downstream application enterprises, which will be beneficial to optimizing the industrial structure and enhancing competitiveness, changing the economic growth model and realizing enterprise industrial upgrading.

[0085] (3) Product production is actively aligned with the national environmental protection and green strategies. Carbon emissions are strictly controlled in the production process. In the selection of raw materials, priority is given to companies with relevant certifications such as carbon footprint certification, bio-based, and sustainable development, and their raw materials are included in the supply chain.

[0086] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A clean latex paint with ultra-low VOC and SVOC emissions. It is characterized in that Includes the following components in percentage by mass: 30-40% water-based acrylic emulsion, 0.6-1.0% surfactant, 0.4-1.0% hydroxyethyl cellulose, 15-30% pigment, 10-20% filler, 1.03-3.1% functional additive, and the balance water; the functional additive is composed of a dispersant, a defoamer, a leveling agent, a bactericide, a mildew preventer and a pH adjuster; The mass content of volatile organic matter in the aqueous acrylic emulsion is less than 100 ppm, and the mass content of semi-volatile organic matter is less than 200 ppm; the minimum film-forming temperature of the aqueous acrylic emulsion is less than 5° C.; the solid content of the aqueous acrylic emulsion is 49-51%; The mass content of volatile organic matter in the surfactant and functional additive is independently lower than 100 ppm, and the mass percentage content of semi-volatile organic matter is independently lower than 1%; The surfactant consists of a first surfactant and a second surfactant; the first surfactant is a branched fatty alcohol alkoxylated surfactant, and the second surfactant is an ethoxylated compound.

2. The odorless latex paint according to claim 1, It is characterized in that The mass content of residual monomers in the aqueous acrylic emulsion is less than 200 ppm; The mass ratio of the first surfactant to the second surfactant is 1:3-4.

3. The odorless latex paint according to claim 1 or 2, It is characterized in that The model of the water-based acrylic emulsion is PLUS 7679; the model of the hydroxyethyl cellulose is B30K; the model of the first surfactant is EH-9; and the model of the second surfactant is EF-90.

4. The odorless latex paint according to claim 1, It is characterized in that The dispersant is sodium salt of acrylic acid homopolymer; the defoamer is mineral oil defoamer; the leveling agent is polyurethane leveling agent; and the pH value regulator is sodium hydroxide solution with a mass concentration of 1-10%.

5. The odorless latex paint according to claim 4, It is characterized in that The mass percentage of the dispersant in the odorless latex paint is 0.3-0.8%, the mass percentage of the defoamer is 0.3-0.8%, the mass percentage of the leveling agent is 0.1-0.5%, the mass percentage of the bactericide is 0.2-0.4%, the mass percentage of the mildewproof agent is 0.1-0.3%, and the mass percentage of the pH value regulator is 0.03-0.3%.

6. The odorless latex paint according to claim 1, 4 or 5, It is characterized in that The model of the dispersant is P30; the model of the defoamer is F210; the model of the leveling agent is U300E; the model of the bactericide is MBS 5050 and / or EG CONC; and the model of the mildewcide is PW-40.

7. The odorless latex paint according to claim 1, It is characterized in that The pigment is titanium dioxide; the mesh number of the titanium dioxide is 500 to 1000 mesh; The filler is heavy calcium and / or calcined kaolin; the mesh number of the heavy calcium is 600-1500 meshes, and the mesh number of the calcined kaolin is 5000-6000 meshes.

8. The odorless latex paint according to claim 7, It is characterized in that The model of the titanium dioxide is R996, the model of the heavy calcium carbonate is JF-1250, and the model of the calcined kaolin is 80L.

9. A method for preparing a clean latex paint with ultra-low VOC and SVOC emissions according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Premixing water, a dispersant, a first surfactant, a defoamer, hydroxyethyl cellulose and a pH regulator to obtain a premix; Dispersing the premix, pigment and filler to obtain a dispersed slurry; The dispersed slurry is mixed with a water-based acrylic emulsion, a leveling agent, a second surfactant, a mildew preventive, and a bactericide to obtain the odorless latex paint with ultra-low VOC and SVOC emissions.

10. The preparation method according to claim 9, It is characterized in that The stirring speed of the premixing is 300-500 rpm; the stirring speed of the dispersing is 700-800 rpm; and the stirring speed of the mixing is 500-700 rpm.

Citation Information

Patent Citations

  • Shell powder aldehyde-resistant photochromic artistic coating and preparation method thereof

    CN110655833A