Graphene-containing water-based coating composition and preparation method thereof

Through pretreatment and hydrothermal conditions, graphene exposing the acyl chloride group reacts with epoxy resin, the problem of poor agglomeration and dispersion of carbon nanotubes is solved, high dispersion and strong interface connection are achieved, and the physical and chemical properties of the coating are significantly improved.

CN119060613AActive Publication Date: 2024-12-03彭建武
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411455403.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-03
Estimated Expiration
2044-10-18

AI Technical Summary

Technical Problem

In the prior art, the agglomeration phenomenon and dispersion of carbon nanotubes in organic matter are poor, resulting in poor conductivity and electromagnetic shielding performance, insufficient reaction between the acid chloride group and the hydroxyl group, and poor modification effect.

Method used

By pretreating graphene to improve its dispersion, and expose the acid chloride group under hydrothermal conditions, it fully reacts with the hydroxyl groups in the epoxy resin to form fully functional graphene, ensuring high dispersion of graphene in the coating Connect with strong interface to improve the physical and chemical properties of the paint.

Benefits of technology

The dispersion and curing reaction of graphene in epoxy resin coatings are significantly improved, the mechanical properties and electrical conductivity of the coating are enhanced, and the physical and chemical properties of the coating are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

According to the graphene-containing water-based coating composition and the preparation method thereof provided by the invention, graphene is subjected to surface modification, so that the dispersity and uniformity of graphene in an epoxy resin coating are remarkably improved, and the physical and chemical properties of the epoxy resin coating are further remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of graphene coating modification, and in particular to a method for improving the chemical properties of epoxy resin coating by using modified graphene. Background Art

[0002] Epoxy resin is a high-performance thermosetting plastic that is widely used in many industries due to its unique chemical structure and properties. Epoxy resin is a high molecular polymer containing more than two epoxy groups, and its molecular structure is defined as (C 11 H 12 O3)n. This substance is usually formed by the condensation of epichlorohydrin with bisphenol A or polyols and belongs to a large class of specific polymers. Among them, bisphenol F epoxy resin is one of the most common epoxy resins. It is made by reacting bisphenol F (a specific type of phenolic compound) with epoxy compounds. Compared with bisphenol A epoxy resin, bisphenol F epoxy resin provides different performance characteristics in certain applications and has better chemical stability and thermal stability.

[0003] Epoxy resin has the following characteristics: (1) Excellent bonding properties: Epoxy resin can form strong bonds with many different types of materials (including metals, glass, wood, etc.), which makes it an ideal choice for manufacturing composite materials and adhesives; (2) High mechanical strength: Cured epoxy resin has high tensile strength, compressive strength and flexural strength, which makes it particularly valuable in structural applications; (3) Excellent chemical resistance: Epoxy resin exhibits good resistance to many chemicals (including acids, bases, solvents, etc.), which makes it used in chemical handling and storage fields; (4) Good electrical insulation properties: Epoxy resin has high electrical insulation and low dielectric constant, which is suitable for Used in electronic and electrical fields, such as insulators, circuit boards, etc.; (5) Heat resistance: Epoxy resin can withstand high operating temperatures, and specially formulated epoxy resin can even maintain its performance unchanged in a continuous high temperature environment; (6) Low shrinkage: During the curing process, the volume shrinkage of epoxy resin is very small, which helps to maintain the dimensional stability and overall strength of the finished product; (7) Customizability: By changing the type and proportion of the curing agent or adding other modifiers, the final performance of the epoxy resin can be adjusted to meet the needs of specific applications; (8) Weather resistance: Epoxy resin has good UV resistance and antioxidant properties, and can be used for a long time in outdoor environments without aging.

[0004] These properties make epoxy resin play an important role in many fields such as aerospace, automobile manufacturing, electronics and electrical, energy equipment, construction and civil engineering. However, the application of epoxy resin also faces some limitations, such as toxicity before curing and sensitivity to certain chemicals, so special attention should be paid to safety when handling and using it.

[0005] Graphene, a simple two-dimensional structure, is composed of carbon atoms. The initial study of this material began during the development of X-ray crystallography. Researchers tried to prepare graphene by chemical exfoliation and vapor deposition, but these methods did not work well, causing many researchers to abandon this research. However, in 2004, Novoselov et al. successfully prepared single-layer graphene for the first time using mechanical exfoliation. This achievement has attracted widespread attention to the unique two-dimensional structure of graphene and has triggered a wave of research and application. Although graphene is separated from graphite, by changing the structure of single-layer graphene, a variety of carbon-based materials with different dimensions can be created. For example, twisting single-layer graphene can generate zero-dimensional fullerenes, one-dimensional carbon nanotubes, or three-dimensional graphite stacks. It is this special atomic structure of single-layer graphene that gives it excellent mechanical, thermal and electrical properties.

[0006] Epoxy resin combined with graphene can significantly improve the performance of the material. Solid polymer, widely used in adhesives, coatings and composite materials. Graphene is a single layer of carbon atoms. Two-dimensional materials composed of honeycomb arrangements are known for their excellent mechanical properties, electrical conductivity and thermal conductivity.

[0007] Advantages of combining epoxy resin and graphene: (1) Enhanced mechanical properties: The addition of graphene can significantly improve the strength and stiffness of epoxy resin-based composites. This is because graphene has an extremely high specific surface area and excellent mechanical properties, which can effectively bear loads and transmit forces through composite materials.

[0008] (2) Improved electrical and thermal conductivity: The addition of graphene can significantly improve the electrical and thermal conductivity of epoxy resin, which is very important for applications requiring electromagnetic shielding and thermal management.

[0009] (3) Increased heat resistance: Graphene can improve the thermal stability of epoxy resin, allowing the composite material to work stably at higher temperatures.

[0010] (4) Improved chemical stability: The addition of graphene can improve the corrosion resistance and chemical stability of epoxy resin composites and extend the service life of the material. Due to these improved properties, epoxy resin / graphene composites have potential applications in many fields, including: (1) Aerospace: Used to manufacture lightweight and high-strength structural parts.

[0011] (2) Automobile: used to improve the performance and durability of automobile parts.

[0012] (3) Electronic products: used in circuit boards and electromagnetic shielding materials to improve heat dissipation performance.

[0013] (4) Energy storage: As electrode materials for supercapacitors and batteries, it improves the performance of energy storage devices.

[0014] There are many examples of high-performance coatings prepared by mixing modified graphene with epoxy resin in the prior art. For example, Tianjin University has disclosed a marine anticorrosion and antifouling coating containing graphene and a preparation method thereof. Graphene with antibacterial function is added to epoxy resin as a filler through surface modification, thereby preparing a nano-composite antifouling coating with antibacterial and corrosion-resistant properties. The present invention adds graphene to epoxy resin as a marine antifouling coating, which will fully combine the excellent properties of the two materials, so that the coating has both antifouling and anticorrosion properties, that is, graphene is compounded with epoxy resin, so that the antibacterial properties of graphene and the anticorrosion properties of epoxy resin are organically combined, thereby developing a new antifouling coating with both anticorrosion and antifouling properties. Graphene modification includes: (1) graphene surface hydroxylation; (2) graphene coupling: surface hydroxylated graphene and N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane (KH-602) are dissolved in deionized water according to the mass ratio of surface hydroxylated graphene to N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane 1:(3-6), ultrasonic dispersion is followed by heating and stirring, centrifugal separation is followed by washing and drying, and grinding is followed to obtain coupled modified graphene, which is specifically carried out according to the following steps: modified graphene and KH602 (N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane) are dissolved in a small amount of deionized water according to the mass ratio of m graphene:mKH-602=1:(3-6); after stirring evenly, ultrasonic dispersion is performed for 30 minutes. The system was heated and stirred at 60°C with a magnetic stirrer for 8 to 10 hours, and the modified graphene was separated by centrifugation, washed 3 times with distilled water and 2 times with ethanol, dried in an oven at 60°C, and ground.

[0015] In addition, the method of chemically modifying polyurethane conductive coating with carbon nanotubes in CN105385330B should be paid special attention to. The method adopts carbon nanotubes grafted with functionalized polyacrylic chloride, and the reaction liquid is grafted with polyurethane resin with hydroxyl group, that is, the remaining acyl chloride group is reacted with polyurethane with hydroxyl group to obtain polyurethane resin chemically modified with carbon nanotubes, and finally the obtained modified polyurethane is mixed with unmodified polyurethane to make coating. This method uses active acyl chloride groups to graft with carbon nanotubes, and then grafts with polyurethane, which ensures the uniformity of dispersion and filling firmness of carbon nanotubes in coating; moreover, it significantly improves the grafting rate of carbon nanotubes, effectively eliminates the agglomeration of carbon nanotubes in organic matter, improves its dispersibility in polyurethane coating and improves the conductivity of coating, and then obtains highly dispersible nano-composite polyurethane coating to prepare modified coating with excellent antistatic performance and electromagnetic shielding performance. Its beneficial effects are described as follows: the method for chemically modifying polyurethane conductive coating with carbon nanotubes is provided, carbon nanotubes treated with functionalization by grafting polyacryl chloride are used, and the reaction liquid is then grafted with polyurethane resin with hydroxyl groups, that is, the remaining acyl chloride groups are used to react with polyurethane with hydroxyl groups to obtain polyurethane resin chemically modified with carbon nanotubes, and finally the obtained modified polyurethane is mixed with unmodified polyurethane to prepare coating. The method uses active acyl chloride groups to graft with carbon nanotubes, and then grafts with polyurethane, which ensures the uniformity of dispersion and filling firmness of carbon nanotubes in coatings; and significantly improves the grafting rate of carbon nanotubes, effectively eliminates the agglomeration of carbon nanotubes in organic matter, improves its dispersibility in polyurethane coatings and improves the conductivity of coatings, thereby obtaining highly dispersible nano-composite polyurethane coatings to prepare modified coatings with excellent antistatic properties and electromagnetic shielding properties. The most serious technical problem of this patent is that the remaining acyl chloride groups are used to react with polyurethane containing hydroxyl groups to obtain polyurethane resin chemically modified with carbon nanotubes. However, it is well known in the art that the remaining acyl chlorides will be completely encapsulated in organic groups and difficult to contact with subsequent hydroxyl groups. In other words, it is difficult to achieve a complete and sufficient reaction of the remaining acyl chloride groups with polyurethane containing hydroxyl groups only through natural reactions, and the modification effect is poor. Summary of the invention

[0016] Based on the above content, firstly, mixed acid is used to pretreat graphene to obtain fluffy graphene with good dispersibility. The fluffy graphene surface contains some functional groups for improving the dispersibility of graphene. Then the surface functional groups react with part of the acyl chloride in the synthesized polymer to complete the polymer grafting. The remaining acyl chloride is fully exposed under hydrothermal conditions and fully reacts with the hydroxyl group in the epoxy resin, and finally the epoxy resin is fully functionalized to form graphene. Due to the encapsulation of the epoxy resin, the fully functionalized graphene will be dispersed to a great extent in the epoxy resin solution used in the subsequent coating preparation process. Under the curing reaction of the curing agent, a highly dispersed graphene epoxy resin coating structure is obtained, thereby significantly improving the physical and chemical properties of the epoxy resin coating.

[0017] A water-based coating composition containing graphene, comprising the following parts by weight: Epoxy resin 40-70 parts; 15-20 parts of modified graphene powder; TBEP plasticizer 2-3 parts; TEGO270 wetting agent 0.5-0.7 parts; BD-3033 leveling agent 0.2-0.3 parts; Acrysol R8 thickener 0.1-0.3 parts; 0.1-0.5 parts of ammonia water; BYK163 dispersant 4-6 parts; Dow Corning AFE-1410 defoamer 0.2-0.5 parts; 30-40 parts of curing agent; 5-15 parts of deionized water.

[0018] The modified graphene powder is prepared by the following steps: (a) pretreatment: placing commercially available graphene powder in a reactor, then adding concentrated nitric acid and concentrated sulfuric acid to form a mixed acid solution, heating to 90-98° C., cooling water to condense and reflux for 4-5 hours, then cooling to room temperature, filtering and washing multiple times, placing the brown graphene solid separation in a refrigerator to freeze for 5-6 hours, and then placing it in a low-temperature vacuum freeze dryer to dry for 6-10 hours, and taking out the fluffy graphene powder.

[0019] (b) Preparation of grafted polymer: 68-90 mg of initiator AIBN and 4-5 ml of acryloyl chloride are dissolved in 10-12 ml of 1,4-dioxane solvent, and then placed in a 60-70 ml reactor. The reactor is dried, nitrogen-filled, and stirred at 60-62° C. for 20-30 hours.

[0020] (c) Modified graphene powder: add 150-170 mg of the graphene powder prepared in step (a) and 100-120 ml of 1,4-dioxane solvent to a zero-moisture reaction metal bottle filled with nitrogen, stir evenly and seal and drop all the polymer prepared in step (b), react at 60-70°C for 36-40 hours, continue to introduce nitrogen, cool naturally, add 220-240 ml of epoxy resin, seal the reactor, use nitrogen to control the pressure of the reaction gas in the metal bottle to 6-7 MPa, turn off the nitrogen introduction, and heat the reactor by program heating, wherein the program heating is to increase the temperature to 95-100°C at a heating rate of 1-2°C, solvent thermal reaction for 24-48 hours, stir the reaction for 48 hours, cool naturally, and take out.

[0021] (d) Post-treatment: The solid liquid is obtained by centrifugation at 8000-9000 rpm, and then washed with acetone and deionized water for multiple times. The solid washings are placed in a refrigerator for 5-6 hours, and then placed in a low-temperature vacuum freeze dryer for 6-10 hours to take out the modified graphene powder.

[0022] The curing agent is a polyamine curing agent.

[0023] Selected from ethylenediamine or diaminodiphenyl sulfone.

[0024] A method for preparing a graphene-containing aqueous coating composition comprises the following steps: (1) Preparation of modified graphene powder; (2) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, Dow Corning AFE-1410 defoaming agent and modified graphene powder were placed in a reaction container according to the ratio, and homogenized at 1200-1400 rpm for 5-10 minutes to obtain a dispersion; (3) Add epoxy resin, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (2), homogenize at 1200-1400 rpm for 5-10 min, add the remaining deionized water, and stir evenly; (4) Continue to add curing agent to step (3), stir and mix thoroughly for 30-40 minutes, and then cure at 30-40°C for 60-90 minutes.

[0025] Modified graphene powder is prepared by the following steps: (a) Pretreatment: Place commercially available graphene powder in a reactor, then add concentrated nitric acid and concentrated sulfuric acid to form a mixed acid solution, heat to 90-98°C, cool water to condense and reflux for 4-5 hours, then cool to room temperature, filter and wash several times, place the brown graphene solid separator in a refrigerator to freeze for 5-6 hours, then put it into a low-temperature vacuum freeze dryer to dry for 6-10 hours, and take out the fluffy graphene powder.

[0026] (b) Preparation of grafted polymer: 68-90 mg of initiator AIBN and 4-5 ml of acryloyl chloride are dissolved in 10-12 ml of 1,4-dioxane solvent, and then placed in a 60-70 ml reactor. The reactor is dried, nitrogen-filled, and stirred at 60-62° C. for 20-30 hours.

[0027] (c) Modified graphene powder: add 150-170 mg of the graphene powder prepared in step (a) and 100-120 ml of 1,4-dioxane solvent to a zero-moisture reaction metal bottle filled with nitrogen, stir evenly and seal and drop all the polymer prepared in step (b), react at 60-70°C for 36-40 hours, continue to introduce nitrogen, cool naturally, add 220-240 ml of epoxy resin organic dispersion, seal the reactor, use nitrogen to control the pressure of the reaction gas in the metal bottle to 6-7 MPa, turn off the nitrogen introduction, and heat the reactor by program heating, wherein the program heating is to increase the temperature to 95-100°C at a heating rate of 1-2°C, solvent thermal reaction for 24-48 hours, stir the reaction for 48 hours, cool naturally, and take out.

[0028] (d) Post-treatment: The solid liquid is obtained by centrifugation at 8000-9000 rpm, and then washed with acetone and deionized water for multiple times. The solid washings are placed in a refrigerator for 5-6 hours, and then placed in a low-temperature vacuum freeze dryer for 6-10 hours to take out the modified graphene powder.

[0029] The epoxy resin dispersion is epoxy resin and 1,4-dioxane solvent in a mass ratio of 1:1.5-2.

[0030] Beneficial technical effects: The epoxy groups modified on the surface of graphene in the present invention can further participate in the curing reaction of the epoxy resin matrix to form a strong interface effect of chemical bond connection, so that the graphene can effectively bear external loads and improve the physical and chemical mechanical properties; (2) the unreacted or buried acyl chloride groups are fully exposed under hydrothermal conditions and fully react with the hydroxyl groups in the epoxy resin, and finally the epoxy resin fully functionalizes the graphene; the fully functionalized graphene will be greatly dispersed in the epoxy resin solution used in the subsequent coating preparation process due to the encapsulation of the epoxy resin, and under the curing reaction of the curing agent, a highly dispersed graphene epoxy resin coating structure is obtained, thereby significantly improving the physical and chemical properties of the epoxy resin coating. DETAILED DESCRIPTION Example 1

[0031] A method for preparing a graphene-containing aqueous coating composition comprises the following steps: (1) Preparation of modified graphene powder.

[0032] (2) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, Dow Corning AFE-1410 defoaming agent and modified graphene powder were placed in a reaction container according to the ratio, and homogenized at 1200 rpm for 5 minutes to obtain a dispersion.

[0033] (3) Add epoxy resin emulsion, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (2), homogenize at 1200 rpm for 5 min, add the remaining deionized water, and stir evenly.

[0034] (4) Continue to add diaminodiphenyl sulfone curing agent to step (3), stir and mix thoroughly for 30 minutes, and then cure at 30°C for 60 minutes.

[0035] The weight proportions of each component in the coating are as follows: 40 parts of epoxy resin emulsion; 15 parts of modified graphene powder; 2 parts of TBEP plasticizer; 0.5 parts of TEGO270 wetting agent; 0.2 parts of BD-3033 leveling agent; 0.1 parts of Acrysol R8 thickener; 0.1 parts of ammonia water; 4 parts of BYK163 dispersant; 0.2 parts of Dow Corning AFE-1410 defoamer; 30 parts of curing agent; and 5 parts of deionized water.

[0036] The modified graphene powder is prepared by the following steps: (a) pretreatment: commercially available graphene powder is placed in a reactor, and then concentrated nitric acid and concentrated sulfuric acid are added to form a mixed acid solution, which is heated to 90°C, cooled with water for condensation and reflux for 4 hours, and then cooled to room temperature. After multiple filtration and washing, the brown graphene solid separation is placed in a refrigerator for 5 hours, and then placed in a low-temperature vacuum freeze dryer for 6 hours to take out the fluffy graphene powder.

[0037] (b) Preparation of grafted polymer: 68 mg of initiator AIBN and 4 ml of acryloyl chloride were dissolved in 10 ml of 1,4-dioxane solvent, and then placed in a 60 ml reactor. The reactor was dried, nitrogen-filled, and stirred at 60° C. for 20-30 hours.

[0038] (c) Modified graphene powder: add 150 mg of the graphene powder prepared in step (a) and 100 ml of 1,4-dioxane solvent to a zero-moisture reaction metal bottle filled with nitrogen, stir evenly and seal and drop all the polymer prepared in step (b), react at 60°C for 36 hours, continue to introduce nitrogen, cool naturally, add 220 ml of epoxy resin organic dispersion, seal the reactor, use nitrogen to control the pressure of the reaction gas in the metal bottle to 6 MPa, turn off the nitrogen introduction, and heat the reactor with a programmed temperature increase, wherein the programmed temperature increase is to increase the temperature to 95°C at a heating rate of 1°C, solvent thermal reaction for 24 hours, stir the reaction for 48 hours, cool naturally, and take out.

[0039] (d) Post-treatment: The solid liquid was obtained by centrifugation at 8000 rpm, and then washed with acetone and deionized water for multiple times. The solid washings were placed in a refrigerator for 5 h, and then placed in a low-temperature vacuum freeze dryer for 6 h to take out the modified graphene powder.

[0040] The epoxy resin organic dispersion is epoxy resin and 1,4-dioxane solvent in a mass ratio of 1:1.5. Example 2

[0041] A method for preparing a graphene-containing aqueous coating composition comprises the following steps: (1) Preparation of modified graphene powder.

[0042] (2) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, Dow Corning AFE-1410 defoaming agent and modified graphene powder were placed in a reaction container according to the ratio, and homogenized at 1300 rpm for 7.5 min to obtain a dispersion.

[0043] (3) Add epoxy resin emulsion, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (2), homogenize at 1300 rpm for 7.5 min, add the remaining deionized water, and stir evenly.

[0044] (4) Continue to add diaminodiphenyl sulfone curing agent to step (3), stir and mix thoroughly for 35 minutes, and then cure at 35°C for 75 minutes.

[0045] The weight proportions of each component in the coating are as follows: 55 parts of epoxy resin emulsion; 17.5 parts of modified graphene powder; 2.5 parts of TBEP plasticizer; 0.6 parts of TEGO270 wetting agent; 0.25 parts of BD-3033 leveling agent; 0.2 parts of Acrysol R8 thickener; 0.3 parts of ammonia water; 5 parts of BYK163 dispersant; 0.35 parts of Dow Corning AFE-1410 defoamer; 35 parts of curing agent; and 10 parts of deionized water.

[0046] The modified graphene powder is prepared by the following steps: (a) pretreatment: commercially available graphene powder is placed in a reactor, and then concentrated nitric acid and concentrated sulfuric acid are added to form a mixed acid solution, which is heated to 95°C, cooled with water for condensation and reflux for 4.5 hours, and then cooled to room temperature. After multiple filtration and washing, the brown graphene solid separation is placed in a refrigerator for 5.5 hours, and then placed in a low-temperature vacuum freeze dryer for 8 hours to take out the fluffy graphene powder.

[0047] (b) Preparation of grafted polymer: 79 mg of initiator AIBN and 4.5 ml of acryloyl chloride were dissolved in 11 ml of 1,4-dioxane solvent and then placed in a 65 ml reactor. The reactor was dried, nitrogen-filled, and stirred at 61° C. for 25 hours.

[0048] (c) Modified graphene powder: add 160 mg of the graphene powder prepared in step (a) and 110 ml of 1,4-dioxane solvent to a zero-moisture reaction metal bottle filled with nitrogen, stir evenly and seal and drop all the polymer prepared in step (b), react at 65°C for 38 hours, continue to introduce nitrogen, cool naturally, add 230 ml of epoxy resin organic dispersion, seal the reactor, use nitrogen to control the pressure of the reaction gas in the metal bottle to 6.5 MPa, turn off the nitrogen introduction, and heat the reactor with a programmed temperature increase, wherein the programmed temperature increase is to increase the temperature to 97.5°C at a heating rate of 1.5°C, perform solvent thermal reaction for 36 hours, stir the reaction for 48 hours, cool naturally, and take out.

[0049] (d) Post-treatment: The solid liquid was obtained by centrifugation at 8500 rpm, and then washed with acetone and deionized water for multiple times. The solid washings were placed in a refrigerator and frozen for 5.5 h, and then placed in a low-temperature vacuum freeze dryer and dried for 8 h to take out the modified graphene powder.

[0050] The epoxy resin organic dispersion is epoxy resin and 1,4-dioxane solvent in a mass ratio of 1:1.75. Example 3

[0051] A method for preparing a graphene-containing aqueous coating composition comprises the following steps: (1) Preparation of modified graphene powder.

[0052] (2) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, Dow Corning AFE-1410 defoaming agent and modified graphene powder were placed in a reaction container according to the ratio, and homogenized at 1400 rpm for 10 min to obtain a dispersion.

[0053] (3) Add epoxy resin emulsion, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (2), homogenize at 1400 rpm for 10 min, add the remaining deionized water, and stir evenly.

[0054] (4) Add diaminodiphenyl sulfone curing agent to step (3), stir and mix thoroughly for 40 minutes, and then cure at 40°C for 90 minutes.

[0055] The weight proportions of each component in the coating are as follows: 70 parts of epoxy resin emulsion; 20 parts of modified graphene powder; 3 parts of TBEP plasticizer; 0.7 parts of TEGO270 wetting agent; 0.3 parts of BD-3033 leveling agent; 0.3 parts of Acrysol R8 thickener; 0.5 parts of ammonia water; 6 parts of BYK163 dispersant; 0.5 parts of Dow Corning AFE-1410 defoamer; 40 parts of curing agent; and 15 parts of deionized water.

[0056] The modified graphene powder is prepared by the following steps: (a) pretreatment: commercially available graphene powder is placed in a reactor, and then concentrated nitric acid and concentrated sulfuric acid are added to form a mixed acid solution, which is heated to 98°C, cooled with water for condensation and reflux for 5 hours, and then cooled to room temperature. After multiple filtration and washing, the brown graphene solid separation is placed in a refrigerator for 6 hours, and then placed in a low-temperature vacuum freeze dryer for 10 hours to take out the fluffy graphene powder.

[0057] (b) Preparation of grafted polymer: 90 mg of initiator AIBN and 5 ml of acryloyl chloride were dissolved in 12 ml of 1,4-dioxane solvent and then placed in a 70 ml reactor. The reactor was dried, nitrogen-filled, and stirred at 62° C. for 30 hours.

[0058] (c) Modified graphene powder: add 170 mg of the graphene powder prepared in step (a) and 120 ml of 1,4-dioxane solvent to a zero-moisture reaction metal bottle filled with nitrogen, stir evenly and seal and drop all the polymer prepared in step (b), react at 70°C for 40 hours, continue to introduce nitrogen, cool naturally, add 240 ml of epoxy resin organic dispersion, seal the reactor, use nitrogen to control the pressure of the reaction gas in the metal bottle to 7 MPa, turn off the nitrogen introduction, and heat the reactor with a programmed temperature increase, wherein the programmed temperature increase is to increase the temperature to 100°C at a heating rate of 2°C, solvent thermal reaction for 48 hours, stir the reaction for 48 hours, cool naturally, and take out.

[0059] (d) Post-treatment: The solid liquid was obtained by centrifugation at 9000 rpm, and then washed with acetone and deionized water for multiple times. The solid washings were placed in a refrigerator and frozen for 6 h, and then placed in a low-temperature vacuum freeze dryer and dried for 10 h to take out the modified graphene powder.

[0060] The epoxy resin organic dispersion is epoxy resin and 1,4-dioxane solvent in a mass ratio of 1:1.5-2.

[0061] Comparative Example 2 A method for preparing a graphene-containing aqueous coating composition comprises the following steps: (1) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, and Dow Corning AFE-1410 defoamer were placed in a reaction container according to the ratio, and homogenized at 1300 rpm for 7.5 min to obtain a dispersion.

[0062] (2) Add epoxy resin, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (1), homogenize at 1300 rpm for 7.5 min, add the remaining deionized water, and stir evenly.

[0063] (4) Add diaminodiphenyl sulfone curing agent to step (3), stir and mix thoroughly for 35 minutes, and then cure at 35°C for 75 minutes.

[0064] The weight proportions of each component in the coating are as follows: 55 parts of epoxy resin; 2.5 parts of TBEP plasticizer; 0.6 parts of TEGO270 wetting agent; 0.25 parts of BD-3033 leveling agent; 0.2 parts of Acrysol R8 thickener; 0.3 parts of ammonia water; 5 parts of BYK163 dispersant; 0.35 parts of Dow Corning AFE-1410 defoamer; 35 parts of curing agent; and 10 parts of deionized water.

[0065] A method for preparing a graphene-containing aqueous coating composition comprises the following steps: (1) Preparation of modified graphene powder.

[0066] (2) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, Dow Corning AFE-1410 defoaming agent and modified graphene powder were placed in a reaction container according to the ratio, and homogenized at 1300 rpm for 7.5 min to obtain a dispersion.

[0067] (3) Add epoxy resin, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (2), homogenize at 1300 rpm for 7.5 min, add the remaining deionized water, and stir evenly.

[0068] (4) Continue to add diaminodiphenyl sulfone curing agent to step (3), stir and mix thoroughly for 35 minutes, and then cure at 35°C for 75 minutes.

[0069] The weight proportions of each component in the coating are as follows: 55 parts of epoxy resin; 17.5 parts of modified graphene powder; 2.5 parts of TBEP plasticizer; 0.6 parts of TEGO270 wetting agent; 0.25 parts of BD-3033 leveling agent; 0.2 parts of Acrysol R8 thickener; 0.3 parts of ammonia water; 5 parts of BYK163 dispersant; 0.35 parts of Dow Corning AFE-1410 defoamer; 35 parts of curing agent; and 10 parts of deionized water.

[0070] The modified graphene powder is prepared by the following steps: (a) pretreatment: commercially available graphene powder is placed in a reactor, and then concentrated nitric acid and concentrated sulfuric acid are added to form a mixed acid solution, which is heated to 95°C, cooled with water for condensation and reflux for 4.5 hours, and then cooled to room temperature. After multiple filtration and washing, the brown graphene solid separation is placed in a refrigerator for 5.5 hours, and then placed in a low-temperature vacuum freeze dryer for 8 hours to take out the fluffy modified graphene powder.

[0071] Comparative Example 3 A method for preparing a graphene-containing aqueous coating composition comprises the following steps: (1) Preparation of modified graphene powder.

[0072] (2) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, Dow Corning AFE-1410 defoaming agent and modified graphene powder were placed in a reaction container according to the ratio, and homogenized at 1300 rpm for 7.5 min to obtain a dispersion.

[0073] (3) Add epoxy resin emulsion, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (2), homogenize at 1300 rpm for 7.5 min, add the remaining deionized water, and stir evenly.

[0074] (4) Add diaminodiphenyl sulfone curing agent to step (3), stir and mix thoroughly for 35 minutes, and then cure at 35°C for 75 minutes.

[0075] The weight proportions of each component in the coating are as follows: 55 parts of epoxy resin emulsion; 17.5 parts of modified graphene powder; 2.5 parts of TBEP plasticizer; 0.6 parts of TEGO270 wetting agent; 0.25 parts of BD-3033 leveling agent; 0.2 parts of Acrysol R8 thickener; 0.3 parts of ammonia water; 5 parts of BYK163 dispersant; 0.35 parts of Dow Corning AFE-1410 defoamer; 35 parts of curing agent; and 10 parts of deionized water.

[0076] The modified graphene powder is prepared by the following steps: (a) pretreatment: commercially available graphene powder is placed in a reactor, and then concentrated nitric acid and concentrated sulfuric acid are added to form a mixed acid solution, which is heated to 95°C, cooled with water for condensation and reflux for 4.5 hours, and then cooled to room temperature. After multiple filtration and washing, the brown graphene solid separation is placed in a refrigerator for 5.5 hours, and then placed in a low-temperature vacuum freeze dryer for 8 hours to take out the fluffy graphene powder.

[0077] (b) Preparation of grafted polymer: 79 mg of initiator AIBN and 4.5 ml of acryloyl chloride were dissolved in 11 ml of 1,4-dioxane solvent and then placed in a 65 ml reactor. The reactor was dried, nitrogen-filled, and stirred at 61° C. for 25 hours.

[0078] (c) Modified graphene powder: Add 160 mg of the graphene powder prepared in step (a) and 110 ml of 1,4-dioxane solvent into a reaction metal bottle with zero moisture and filled with nitrogen. After stirring evenly, seal and drop all the polymer prepared in step (b). After reacting at 65°C for 38 hours, continue to introduce nitrogen. After cooling naturally, add 230 ml of epoxy resin organic dispersion, stir and react for 48 hours, cool naturally, and take out.

[0079] (d) Post-treatment: The solid liquid was obtained by centrifugation at 8500 rpm, and then washed with acetone and deionized water for multiple times. The solid washings were placed in a refrigerator and frozen for 5.5 h, and then placed in a low-temperature vacuum freeze dryer and dried for 8 h to take out the modified graphene powder.

[0080] The epoxy resin organic dispersion is epoxy resin and 1,4-dioxane solvent in a mass ratio of 1:1.75.

[0081] The physical and chemical properties of Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested, and the tests mainly focused on tensile strength, elastic modulus, tensile strain at break, flexural strength, flexural modulus and impact strength.

[0082]

[0083] Comparative Example 1 is a blank example, Comparative Example 2 is graphene that has only been acid-modified, and Comparative Example 3 is similar to CN105385330B, which is an epoxy resin-modified graphene powder that has not been hydrothermally assisted. The physicochemical properties of Example 2 are significantly better than those of Comparative Examples 1-3, and the reasons may be as follows: (1) The epoxy groups modified on the surface of graphene can further participate in the curing reaction of the epoxy resin matrix to form a strong interface effect of chemical bond connection, so that the graphene can effectively carry external loads and improve the physicochemical mechanical performance; (2) The unreacted or buried acyl chloride groups are fully exposed under hydrothermal conditions and fully react with the hydroxyl groups in the epoxy resin, and finally realize the fully functionalized graphene of the epoxy resin; the fully functionalized graphene will be greatly dispersed in the epoxy resin solution used in the subsequent coating preparation process due to the encapsulation of the epoxy resin, and under the curing reaction of the curing agent, a highly dispersed graphene epoxy resin coating structure is obtained, thereby significantly improving the physicochemical properties of the epoxy resin coating.

[0084] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based coating composition containing graphene, Features The weight parts are as follows: 40-70 parts of epoxy resin emulsion; 15-20 parts of modified graphene powder; TBEP plasticizer 2-3 parts; TEGO270 wetting agent 0.5-0.7 parts; BD-3033 leveling agent 0.2-0.3 parts; Acrysol R8 thickener 0.1-0.3 parts; 0.1-0.5 parts of ammonia water; BYK163 dispersant 4-6 parts; Dow Corning AFE-1410 defoamer 0.2-0.5 parts; 30-40 parts of curing agent; 5-15 parts of deionized water.

2. A graphene-containing aqueous coating composition according to claim 1, Features The modified graphene powder is prepared by the following steps: Prepared to obtain: (a) Pretreatment: Place commercially available graphene powder in a reactor, then add concentrated nitric acid and concentrated sulfuric acid to form a mixed acid solution, heat to 90-98°C, cool water to condense and reflux for 4-5 hours, then cool to room temperature, filter and wash multiple times, place the brown graphene solid separation in a refrigerator to freeze for 5-6 hours, then put it into a low-temperature vacuum freeze dryer to dry for 6-10 hours, and take out the fluffy graphene powder; (b) Preparation of grafted polymer: 68-90 mg of initiator AIBN and 4-5 ml of acryloyl chloride are dissolved in 10-12 ml of 1,4-dioxane solvent, and then placed in a 60-70 ml reactor. The reactor is dried, nitrogen-filled, and stirred at 60-62° C. for 20-30 hours. (c) Modified graphene powder: add 150-170 mg of the graphene powder prepared in step (a) and 100-120 ml of 1,4-dioxane solvent to a zero-moisture metal reaction bottle filled with nitrogen, stir evenly and seal and drop all the polymer prepared in step (b), react at 60-70°C for 36-40 hours, continue to introduce nitrogen, cool naturally, add 220-240 ml of epoxy resin organic dispersion, seal the reactor, use nitrogen to control the pressure of the reaction gas in the metal bottle to 6-7 MPa, turn off the nitrogen introduction, and heat the reactor with a programmed temperature increase, wherein the programmed temperature increase is to increase the temperature to 95-100°C at a heating rate of 1-2°C, solvent thermal reaction for 24-48 hours, stir the reaction for 48 hours, cool naturally, and take out; (d) Post-treatment: The solid liquid is obtained by centrifugation at 8000-9000 rpm, and then washed with acetone and deionized water for multiple times. The solid washings are placed in a refrigerator for 5-6 hours, and then placed in a low-temperature vacuum freeze dryer for 6-10 hours to take out the modified graphene powder.

3. A graphene-containing aqueous coating composition according to claim 1, Features The curing agent is a polyamine curing agent.

4. A graphene-containing aqueous coating composition according to claim 3, Its characteristics are The curing agent is selected from ethylenediamine or diaminodiphenyl sulfone.

5. A method for preparing a water-based coating composition containing graphene, Features The steps include: (1) Preparation of modified graphene powder; (2) Deionized water, part of TEGO270 wetting agent, part of BYK163 dispersant, Dow Corning AFE-1410 defoaming agent and modified graphene powder were placed in a reaction container according to the ratio, and homogenized at 1200-1400 rpm for 5-10 minutes to obtain a dispersion; (3) Add epoxy resin emulsion, TBEP plasticizer, BD-3033 leveling agent, remaining TEGO270 wetting agent, remaining BYK163 dispersant, Acrysol R8 thickener, and aqueous ammonia to the dispersion obtained in step (2), homogenize at 1200-1400 rpm for 5-10 min, add remaining deionized water, and stir evenly; (4) Continue to add curing agent to step (3), stir and mix thoroughly for 30-40 minutes, and then cure at 30-40°C for 60-90 minutes.

6. A method for preparing a graphene-containing aqueous coating composition according to claim 5, Features Modified graphene powder is prepared by the following steps: (a) Pretreatment: Place commercially available graphene powder in a reactor, then add concentrated nitric acid and concentrated sulfuric acid to form a mixed acid solution, heat to 90-98°C, cool water to condense and reflux for 4-5 hours, then cool to room temperature, filter and wash multiple times, place the brown graphene solid separation in a refrigerator to freeze for 5-6 hours, then put it into a low-temperature vacuum freeze dryer to dry for 6-10 hours, and take out the fluffy graphene powder; (b) Preparation of grafted polymer: 68-90 mg of initiator AIBN and 4-5 ml of acryloyl chloride are dissolved in 10-12 ml of 1,4-dioxane solvent, and then placed in a 60-70 ml reactor. The reactor is dried, nitrogen-filled, and stirred at 60-62° C. for 20-30 hours. (c) Modified graphene powder: add 150-170 mg of the graphene powder prepared in step (a) and 100-120 ml of 1,4-dioxane solvent to a zero-moisture metal reaction bottle filled with nitrogen, stir evenly and seal and drop all the polymer prepared in step (b), react at 60-70°C for 36-40 hours, continue to introduce nitrogen, cool naturally, add 220-240 ml of epoxy resin organic dispersion, seal the reactor, use nitrogen to control the pressure of the reaction gas in the metal bottle to 6-7 MPa, turn off the nitrogen introduction, and heat the reactor with a programmed temperature increase, wherein the programmed temperature increase is to increase the temperature to 95-100°C at a heating rate of 1-2°C, solvent thermal reaction for 24-48 hours, stir the reaction for 48 hours, cool naturally, and take out; (d) Post-treatment: The solid liquid is obtained by centrifugation at 8000-9000 rpm, and then washed with acetone and deionized water for multiple times. The solid washings are placed in a refrigerator for 5-6 hours, and then placed in a low-temperature vacuum freeze dryer for 6-10 hours to take out the modified graphene powder.

7. A method for preparing a graphene-containing aqueous coating composition according to claim 6, Features The epoxy resin organic dispersion is epoxy resin and 1,4-dioxane solvent in a mass ratio of 1:1.5-2.

Citation Information

Patent Citations

  • Preparation method for copolymerization living polymer modified graphene oxide

    CN105199436A

  • Graphene epoxy compound material for electric automobile driving module and preparation method

    CN108102300A

  • Preparation method of water-based paint

    CN115612376A