Modified waterproof coating and preparation method thereof

By modifying the isocyanate prepolymer, fluorine-containing compounds and nano-inorganic materials in the waterproof coating formula, a dense network structure is formed, which solves the problem of oxidation and degradation of traditional coatings under ultraviolet light, and significantly improves the durability of the coating film and Waterproof performance.

CN119060627AInactive Publication Date: 2024-12-03HEBEI YUYANGZELI WATERPROOF MATERIAL
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411375221.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional single-component polyurethane waterproof coatings are prone to oxidation and degradation under ultraviolet radiation, resulting in the gradual decline of the waterproof function of the coating film and poor durability.

Method used

Using modified waterproof coating formulations, including isocyanate prepolymers, fluorine-containing compounds, nano-inorganic materials, antioxidants, plasticizers and fillers, a dense network structure is formed through high shear mixing and stirring processes to enhance the stability of the coating film and Waterproof performance.

Benefits of technology

Effectively prevent the oxidative degradation of polyurethane groups, extend the service life of the coating, improve the mechanical properties, compressive strength and wear resistance of the coating film, reduce ultraviolet damage, maintain good adhesion and elasticity, and significantly improve waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof coatings, and discloses a modified waterproof coating and a preparation method thereof. The modified waterproof coating is prepared from the following components in parts by weight: 100 parts of isocyanate prepolymer, 5 to 30 parts of fluorine-containing compound, 5 to 20 parts of nano inorganic material, 0.5 to 5 parts of antioxidant, 5 to 20 parts of plasticizer, 10 to 50 parts of filler and 0.5 to 3 parts of defoaming agent. According to the modified waterproof coating disclosed by the invention, through the synergistic effect of multiple components, the durability, physical properties and environmental adaptability of the coating are remarkably improved, and the problem that the traditional coating is insufficient in durability in ultraviolet and oxidation environments is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of waterproof coatings, and in particular to a modified waterproof coating and a preparation method thereof. Background Art

[0002] As an important material in the field of building waterproofing, single-component moisture-curing polyurethane waterproof coating relies on the cross-linking and curing reaction between the isocyanate group (-NCO) in the polyurethane prepolymer and the moisture in the air to form a continuous and dense waterproof film. This type of coating has the characteristics of easy construction, environmental protection and solvent-free, and is therefore widely used under certain humidity conditions.

[0003] Isocyanate components in traditional one-component polyurethane waterproof coatings, such as TDI (toluene diisocyanate) and MDI (4,4'-diphenylmethane diisocyanate), can effectively provide the basis for the curing reaction, but are prone to oxidative degradation under long-term exposure to ultraviolet radiation. Ultraviolet radiation will cause changes in the chemical structure of the polyurethane coating, causing its surface to gradually turn yellow, powdery, and cracked, leading to the gradual decline of the coating's waterproof function. Specifically, ultraviolet radiation causes the isocyanate group to undergo a photochemical reaction with oxygen or moisture in the environment to generate amine compounds. Amine compounds continue to react with isocyanates to generate urea structures. This process not only changes the original cross-linking network, causing the molecular chain to break, but also reduces the mechanical strength and waterproof properties of the coating. Summary of the invention

[0004] In view of this, the present invention proposes a modified waterproof coating and a preparation method thereof, aiming to solve the problem in the current technology that the isocyanate component in the single-component polyurethane waterproof coating is prone to oxidative degradation and the coating has poor durability.

[0005] On the one hand, a modified waterproof coating proposed by the present invention comprises the following components in parts by weight:

[0006] 100 parts by weight of isocyanate prepolymer, 5-30 parts by weight of fluorine-containing compound, 5-20 parts by weight of nano inorganic material, 0.5-5 parts by weight of antioxidant, 5-20 parts by weight of plasticizer, 10-50 parts by weight of filler and 0.5-3 parts by weight of defoamer.

[0007] Preferably, the isocyanate prepolymer is obtained by reacting hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate with a polyol.

[0008] Preferably, the polyol is polypropylene glycol or polytetramethylene glycol;

[0009] The molecular weight of the polypropylene glycol ester is 1000-4000, and the molecular weight of the polytetrahydrofuran diol is 500-2000.

[0010] Preferably, the fluorine-containing compound is perfluorooctyl phosphate or perfluorooctyl ethanol;

[0011] The fluorine content of the fluorine-containing compound is greater than 60%, and the molecular weight is 400-600.

[0012] Preferably, the nano inorganic material is nano silicon dioxide and / or nano zinc oxide.

[0013] Preferably, the antioxidant is any one of TINUVIN 144, TINUVIN 622, BHT and BHA.

[0014] Preferably, the plasticizer is dioctyl phthalate, the filler is silicon dioxide, and the defoamer is TEGO Foamex K3.

[0015] On the other hand, the present invention also provides a method for preparing a modified waterproof coating, comprising the following steps:

[0016] Mix hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate with polypropylene glycol and polytetramethylene glycol, and react at 60-80°C for 4-8h. When the conversion rate of the active groups of hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate is at least 80% or the reaction time is reached, terminate the reaction to obtain an isocyanate prepolymer;

[0017] Adding the nano inorganic material into ethanol or xylene and dispersing it using a high shear mixer;

[0018] In a reaction kettle, the isocyanate prepolymer, the fluorine-containing compound, the nano inorganic material, and a plasticizer, a filler and a defoamer are added in sequence, and the stirring speed is maintained at 300-500 rpm for 30 minutes;

[0019] Gradually add antioxidants, and continue stirring at a stirring speed of 300-500 rpm for 10-15 minutes; after standing for 2-4 hours, filter through an 80-mesh sieve to remove large solid particles to obtain a modified waterproof coating.

[0020] Furthermore, when preparing the isocyanate prepolymer, the added mass ratio of hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate to polypropylene glycol diacid or polytetramethylene glycol is 1:1.2-1.5.

[0021] Furthermore, the high shear mixer is set to have a rotation speed of 1000-5000RPM, a feed rate of 1-5kg / min, and a dispersion time of 30-60min.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The antioxidant added to the modified waterproof coating can effectively capture the free radicals generated in the coating and prevent the oxidative degradation of the polyurethane groups, thereby extending the service life of the coating. This mechanism inhibits the oxidation chain reaction caused by ultraviolet rays by reducing the chemical reaction rate.

[0024] Perfluorooctyl phosphate and perfluorooctyl ethanol have strong UV shielding effects. The introduction of fluorinated compounds not only provides a physical barrier to slow down the damage of ultraviolet rays to polyurethane, but also chemically enhances the stability of the coating. The excellent moisture resistance and hydrophobicity of fluorinated materials reduce the penetration of water and reduce the possibility of photochemical reactions caused by ultraviolet rays.

[0025] The addition of nano-silicon dioxide and nano-zinc oxide improves the mechanical properties and weather resistance of the coating. The high specific surface area of ​​the nanomaterials interacts with the matrix of the coating to form a denser network structure, thereby improving the tensile strength, compressive strength and wear resistance of the coating. In addition, nanomaterials can also effectively block ultraviolet rays, further improving the anti-ultraviolet ability of the waterproof coating.

[0026] The addition of dioctyl phthalate as a plasticizer enhances the flexibility and crack resistance of the coating, making the coating easier to handle during construction and reducing the brittleness of the film after drying. Even under environmental changes, the coating can maintain good adhesion and elasticity to prevent cracking and peeling. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] As mentioned in the background technology, traditional one-component moisture-curing polyurethane waterproof coatings rely on isocyanate groups (-NCO) to cross-link with moisture in the air to form a dense waterproof film. Although these coatings are convenient and environmentally friendly in construction, they face serious degradation problems when exposed to ultraviolet radiation for a long time. Ultraviolet radiation will cause the surface of the coating to gradually turn yellow, powder and crack, which will seriously reduce the waterproof performance of the coating. This process is mainly caused by the following aspects:

[0029] Chemical structure changes: UV rays will cause isocyanate groups to react with oxygen or moisture to generate amine compounds, which then react with isocyanate to form urea structures. This change not only damages the original cross-linked network, but also breaks the molecular chains, reducing the mechanical strength of the coating.

[0030] Physical performance degradation: The gradual aging of the coating film causes its waterproof function to gradually weaken, which is extremely detrimental to the protection of buildings and other infrastructure.

[0031] In some embodiments of the present invention, the introduction of antioxidants into the modified waterproof coating can effectively capture and neutralize the free radicals generated in the coating and inhibit the oxidative degradation of the polyurethane group. The oxidation chain reaction caused by ultraviolet radiation is the main reason for the decline in coating performance. By reducing the chemical reaction rate, the antioxidant significantly extends the service life of the coating. This mechanism not only enhances the stability of the coating, but also maintains its excellent mechanical properties and waterproof function. The introduction of fluorinated compounds such as perfluorooctyl phosphate and perfluorooctyl ethanol provides a stronger ultraviolet shielding effect for the modified waterproof coating. These materials slow down the damage of ultraviolet rays to polyurethane by forming a physical barrier, while chemically enhancing the stability of the coating. The good hydrophobicity and moisture resistance of fluorinated compounds can effectively reduce the penetration of water, thereby reducing the occurrence of photochemical reactions caused by ultraviolet rays. Through effective shielding and chemical stability, these fluorinated materials provide lasting protection for the waterproof coating. The addition of nano-silicon dioxide and nano-zinc oxide significantly improves the mechanical properties and weather resistance of the modified waterproof coating. Nanomaterials have a high specific surface area and can form a denser network structure with the coating matrix, thereby improving the tensile strength, compressive strength and wear resistance of the coating. In addition, nano zinc oxide performs well in ultraviolet absorption. While effectively blocking ultraviolet rays, it also improves the anti-ultraviolet ability of the coating, further protecting the chemical structure of the coating from damage. The addition of dioctyl phthalate as a plasticizer improves the flexibility and crack resistance of the coating, making the modified waterproof coating easier to operate during construction. This improvement can also effectively reduce the brittleness of the film after the coating dries, ensuring that the coating can maintain good adhesion and elasticity even under environmental changes, preventing cracking and peeling. The introduction of plasticizers finds a good balance between improving operability and long-term performance.

[0032] The following will be described in conjunction with embodiments.

[0033] Example 1

[0034] Isocyanate prepolymer: 100 parts by weight

[0035] Obtained by the reaction of hexamethylene diisocyanate and polypropylene glycol ester (both with molecular weight of 3000).

[0036] Fluorine-containing compound: 10 parts by weight, perfluorooctyl phosphate, fluorine content of 70%, molecular weight of 500.

[0037] Nano inorganic material: 15 parts by weight, nano silicon dioxide, average particle size 20 nanometers.

[0038] Antioxidant: 1 part by weight, TINUVIN 144 is selected.

[0039] Plasticizer: 10 parts by weight, dioctyl phthalate is selected.

[0040] Filler: 30 parts by weight, selected from silicon dioxide, with a particle size of 10 microns.

[0041] Defoaming agent: 2 parts by weight, model TEGO Foamex K3.

[0042] Preparation steps:

[0043] In a reaction kettle, 100 parts by weight of hexamethylene diisocyanate and 150 parts by weight of polypropylene glycol diol were mixed and reacted at 60° C. for 6 hours. The conversion rate of active groups reached 85%, thereby obtaining an isocyanate prepolymer.

[0044] 15 parts by weight of nano-silicon dioxide were added to 50 parts by weight of xylene and dispersed using a high shear mixer with a rotation speed set to 3000 RPM for 45 minutes.

[0045] Isocyanate prepolymer, 10 parts by weight of perfluorooctyl phosphate, dispersed nano-silica, 10 parts by weight of dioctyl phthalate, 30 parts by weight of silica and 2 parts by weight of TEGO Foamex K3 were added to the reaction kettle in sequence, and the stirring speed was maintained at 400 rpm for 30 minutes.

[0046] 1 part by weight of TINUVIN 144 was gradually added, and the stirring speed was maintained at 400 rpm for 10 minutes.

[0047] After standing for 2 hours, the large solid particles were removed by filtration through an 80-mesh sieve to obtain a modified waterproof coating.

[0048] Example 2

[0049] Isocyanate prepolymer: 100 parts by weight

[0050] Obtained by the reaction of 4,4'-diphenylmethane diisocyanate and polytetramethylene glycol (molecular weight 1500).

[0051] Fluorine-containing compound: 15 parts by weight, perfluorooctylethanol, fluorine content of 65%, molecular weight of 450.

[0052] Nano inorganic material: 10 parts by weight, nano zinc oxide with an average particle size of 30 nanometers.

[0053] Antioxidant: 2 parts by weight, BHT is selected.

[0054] Plasticizer: 10 parts by weight, dioctyl phthalate is selected.

[0055] Filler: 40 parts by weight, selected from silicon dioxide, with a particle size of 20 microns.

[0056] Defoaming agent: 2 parts by weight, model TEGO Foamex K3.

[0057] Preparation steps:

[0058] In a reaction kettle, 100 parts by weight of 4,4'-diphenylmethane diisocyanate and 120 parts by weight of polytetrahydrofuran diol were mixed and reacted at 75°C for 5 hours. When the conversion rate of active groups reached 90%, an isocyanate prepolymer was obtained.

[0059] 10 parts by weight of nano zinc oxide was added to 60 parts by weight of ethanol and dispersed using a high shear mixer with a rotation speed set to 2000 RPM for 35 minutes.

[0060] Isocyanate prepolymer, 15 parts by weight of perfluorooctylethanol, dispersed nano zinc oxide, 10 parts by weight of dioctyl phthalate, 40 parts by weight of silicon dioxide and 2 parts by weight of TEGO Foamex K3 were added to the reaction kettle in sequence, and the stirring speed was maintained at 350 rpm for 30 minutes.

[0061] 2 parts by weight of BHT were gradually added, and the stirring speed was maintained at 350 rpm for 15 minutes.

[0062] After standing for 3 hours, the large solid particles were removed by filtration through an 80-mesh sieve to obtain a modified waterproof coating.

[0063] Example 3

[0064] Isocyanate prepolymer: 100 parts by weight

[0065] Obtained by the reaction of hexamethylene diisocyanate and polypropylene glycol ester (molecular weight 2000);

[0066] Fluorine-containing compound: 20 parts by weight, perfluorooctyl phosphate, with a fluorine content of 68% and a molecular weight of 550.

[0067] Nano inorganic material: 15 parts by weight, nano silicon dioxide (average particle size 10 nanometers) is selected.

[0068] Antioxidant: 3 parts by weight, TINUVIN 622 is selected.

[0069] Plasticizer: 15 parts by weight, dioctyl phthalate is selected.

[0070] Filler: 30 parts by weight, silicon dioxide (particle size 5 microns).

[0071] Defoaming agent: 1.5 parts by weight, model TEGO Foamex K3.

[0072] Preparation steps:

[0073] In a reaction kettle, 100 parts by weight of hexamethylene diisocyanate and 120 parts by weight of polypropylene glycol diol were mixed and reacted at 70° C. for 6 hours. When the conversion rate of active groups reached 80%, an isocyanate prepolymer was obtained.

[0074] 15 parts by weight of nano-silicon dioxide were added to 50 parts by weight of xylene and dispersed using a high shear mixer with a rotation speed set to 4000 RPM for 40 minutes.

[0075] Isocyanate prepolymer, 20 parts by weight of perfluorooctyl phosphate, dispersed nano-silica, 15 parts by weight of dioctyl phthalate, 30 parts by weight of silica and 1.5 parts by weight of TEGOFoamex K3 were added to the reaction kettle in sequence, and the stirring speed was maintained at 300 rpm for 30 minutes.

[0076] 3 parts by weight of TINUVIN 622 were gradually added, and the stirring speed was maintained at 300 rpm for 15 minutes.

[0077] After standing for 2 hours, the large solid particles were removed by filtration through an 80-mesh sieve to obtain a modified waterproof coating.

[0078] Comparative Example 1

[0079] The difference between this comparative example and Example 1 is that the fluorine-containing compound in this comparative example is perfluorooctyl phosphate.

[0080] Comparative Example 2

[0081] The difference between this comparative example and Example 2 is that the nano inorganic material in this comparative example is nano alumina.

[0082] Comparative Example 3

[0083] The difference between this comparative example and Example 3 is that the isocyanate prepolymer is obtained by reacting toluene diisocyanate and polypropylene glycol ester (molecular weight 3000).

[0084] The performance of Examples 1-3 and Comparative Examples 1-3 was tested, and the test data are shown in Table 1. The specific test method is:

[0085] 1. Tensile strength (MPa)

[0086] Standard: ASTM D638 or ISO527

[0087] Equipment: Tensile testing machine

[0088] Steps: Prepare a standard specimen (usually in the shape of a dog tooth or rectangle). Clamp the specimen into the tensile testing machine and record the initial length of the specimen. Stretch the specimen at a certain speed until it breaks. Record the maximum tensile force and the fracture area of ​​the specimen, and calculate the tensile strength (MPa) = maximum tensile force (N) / fracture area (mm²).

[0089] 2. Elongation at break (%)

[0090] Standard: ASTM D638

[0091] Procedure: While conducting the tensile test, record the breaking length of the specimen. Calculate the breaking elongation (%) = [(breaking length - initial length) / initial length] × 100.

[0092] 3. Shear strength (MPa)

[0093] Standard: ASTM D1002

[0094] Procedure: Prepare two specimens, apply adhesive to each and cure under standard conditions. Place the specimen in a shear tester and record the applied shear force. Shear strength (MPa) = maximum applied shear force (N) / shear area (mm²).

[0095] 4. Water resistance (24 hours)

[0096] Standard: ASTM D570

[0097] Procedure: Place the coating sample in water and soak for 24 hours. Take out the sample, wipe off the water, and weigh it to obtain the weight difference before and after soaking. Calculate the water absorption rate (%) = [(weight after soaking - initial weight) / initial weight] × 100.

[0098] 5. UV aging resistance (%)

[0099] Standard: ASTM G154

[0100] Steps: Place the sample in a UV aging tester and irradiate it according to the predetermined time and intensity.

[0101] Regularly measure the changes in the appearance and performance of the coating film. Calculate the UV aging resistance rate (%) = [(strength of unaged sample - strength of aged sample) / strength of unaged sample] × 100%.

[0102] 6. Hardness (Shore A)

[0103] Standard: ASTMD2240

[0104] Steps: Apply the hammer of the Shore hardness tester vertically to the surface of the sample. Read the value of the hardness tester and record the hardness (Shore A) value.

[0105] 7. Moisture permeability (g / m²·24h)

[0106] Standard: ASTM E96

[0107] Steps: Prepare the sample under standard conditions and seal it in the moisture permeability test device. Measure the amount of water vapor passing through in 24 hours (g). Calculate the moisture permeability (g / m²·24h) = the amount of water vapor passing through in 24 hours / sample area.

[0108] 8. Color change (ΔE)

[0109] Standard:CIEDE2000

[0110] Steps: Record the color values ​​(L*, a*, b*) of the unaged sample. After the sample is aged by UV, measure the color value again. Calculate the color change :

[0111] ;

[0112] Among them, ΔL*, Δa*, and Δb* are the changes of L*, a*, and b* before and after aging, respectively.

[0113] Table 1

[0114]

[0115] As can be seen from the table above: in the comparison of the modified waterproof coating examples and comparative examples, we mainly focus on the changes in multiple performance indicators, including tensile strength, elongation at break, shear strength, water resistance, UV aging resistance, hardness, moisture permeability and color change, etc. Through data analysis, we can explore the reasons for these performance changes from a mechanistic perspective and the impact on their application areas.

[0116] Tensile strength (MPa)

[0117] Example 1: 12.5, Example 2: 11.8, Example 3: 13.0, Comparative Example 1: 10.0, Comparative Example 2: 9.5, Comparative Example 3: 10.2;

[0118] Tensile strength is an important indicator for evaluating the ability of coating materials to withstand tensile forces. The tensile strength of the embodiments is between 11.8MPa and 13.0MPa, showing a high degree of molecular chain crosslinking. This crosslinked structure allows the material to disperse stress during stretching and avoid local overload. The tensile strength of the comparative example is significantly reduced, mainly because traditional single-component polyurethane coatings are prone to oxidative degradation under ultraviolet radiation. Ultraviolet rays can cause photochemical reactions of isocyanate groups in the coating film, generate urea structures and cause the breakage of molecular chains, thereby reducing the strength of the material.

[0119] Elongation at break (%)

[0120] Example 1: 300, Example 2: 290, Example 3: 310, Comparative Example 1: 240, Comparative Example 2: 220, Comparative Example 3: 230;

[0121] The elongation at break reflects the flexibility and ductility of the material. The elongation of the embodiment reaches 290%-310%, indicating that it has good toughness and is suitable for dynamic stress environment. On the contrary, the elongation at break of the comparative example is significantly reduced, because the degradation of the cross-linked structure caused by ultraviolet rays leads to a decrease in the toughness of the material. In addition, the lower elongation at break also affects the stability of the material under temperature changes, thereby affecting its long-term performance.

[0122] Shear strength(MPa)

[0123] Example 1: 8.0, Example 2: 7.8, Example 3: 7.9, Comparative Example 1: 5.5, Comparative Example 2: 5.8, Comparative Example 3: 6.1;

[0124] Shear strength is used to evaluate the resistance of coatings to shear forces. The shear strength of the examples (7.8-8.0 MPa) is significantly higher than that of the comparative examples (5.5-6.1 MPa), which is closely related to the chemical structure optimization of the modified polyols and other additives used in the examples. The modified polyurethane coating exhibits better durability in chemical crosslinking and network structure, while the comparative example material gradually relaxes its structure under long-term ultraviolet exposure, resulting in decreased shear performance.

[0125] Water resistance (24 hours)

[0126] Example 1: no penetration, Example 2: no penetration, Example 3: no penetration, Comparative Example 1: penetration, Comparative Example 2: penetration, Comparative Example 3: no penetration;

[0127] Water resistance is an important performance index of waterproof coatings. The examples all show the excellent performance of "no penetration". This shows that the surface is dense and not easily penetrated by water, which ensures its waterproof effect. The penetration phenomenon of the materials in the comparative examples is mainly due to the change of their chemical structure under ultraviolet radiation, which leads to the damage of the surface microstructure and the increase of pores, reducing the waterproof performance of the materials.

[0128] UV aging resistance (%)

[0129] Example 1: 90, Example 2: 85, Example 3: 92, Comparative Example 1: 60, Comparative Example 2: 55, Comparative Example 3: 67;

[0130] The UV aging resistance directly affects the long-term stability of the coating under sunlight. The UV aging resistance of the embodiment is as high as 85%-92%, indicating that the material has strong resistance to ultraviolet rays and can effectively inhibit oxidative degradation caused by photochemical reactions. In contrast, the UV aging resistance of the comparative example is significantly reduced, mainly because the isocyanate groups in traditional polyurethane coatings are prone to react under ultraviolet rays to generate low molecular weight products, resulting in embrittlement and yellowing of the coating surface.

[0131] Hardness (Shore A)

[0132] Example 1: 81, Example 2: 79, Example 3: 77, Comparative Example 1: 72, Comparative Example 2: 77, Comparative Example 3: 84;

[0133] Hardness is an important indicator of the physical properties of coatings. The hardness of the examples is relatively stable and high, showing good mechanical properties. The hardness of the comparative examples fluctuates greatly, especially comparative example 1 (72), which is relatively low, due to the insufficient degree of crosslinking and durability of the materials. The low hardness makes the coating film prone to deformation or cracking in actual use.

[0134] Moisture permeability (g / m²·24h)

[0135] Example 1: 1.2, Example 2: 1.0, Example 3: 1.1, Comparative Example 1: 1.5, Comparative Example 2: 1.6, Comparative Example 3: 1.7;

[0136] Moisture permeability is an important indicator for evaluating the moisture resistance of materials. The moisture permeability of the embodiment (1.0-1.2) is significantly lower than that of the comparative example (1.5-1.7). This shows that the coating of the embodiment has excellent moisture resistance and is suitable for use in humid environments. The higher moisture permeability of the comparative example is due to the degradation of its coating structure and the increase in porosity, which leads to enhanced water permeability and affects the waterproof effect.

[0137] Color change (ΔE)

[0138] Example 1: 2.0, Example 2: 2.5, Example 3: 1.8, Comparative Example 1: 5.1, Comparative Example 2: 4.8, Comparative Example 3: 4.1;

[0139] The color change (ΔE) reflects the appearance stability of the material under ultraviolet irradiation. The ΔE value of the embodiment is relatively low (1.8-2.5), indicating that its color change under light conditions is not obvious and is suitable for long-term use. The ΔE value of the comparative example is higher (4.1-5.1), indicating that its surface has obvious color change, which is mainly due to the chemical reaction caused by ultraviolet rays, which degrades the surface pigment of the material, affecting the appearance and service life of the material.

[0140] Through comprehensive analysis of various performance indicators of the embodiments and comparative examples, we can clearly conclude that the modified waterproof coating has shown significant advantages in multiple performance aspects. These advantages are mainly attributed to the optimization of its molecular chain, the improvement of the degree of cross-linking and the enhancement of environmental resistance, which enables the material to effectively resist ultraviolet rays, moisture and mechanical stress in practical applications.

[0141] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A modified waterproof coating, characterized in that: The composition comprises the following components in parts by weight: 100 parts by weight of isocyanate prepolymer, 5-30 parts by weight of fluorine-containing compound, 5-20 parts by weight of nano inorganic material, 0.5-5 parts by weight of antioxidant, 5-20 parts by weight of plasticizer, 10-50 parts by weight of filler and 0.5-3 parts by weight of defoamer.

2. A modified waterproof coating according to claim 1, characterized in that: The isocyanate prepolymer is obtained by reacting hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate with polyol.

3. A modified waterproof coating according to claim 2, characterized in that: The polyol is polypropylene glycol ester or polytetramethylene glycol; The molecular weight of the polypropylene glycol ester is 1000-4000, and the molecular weight of the polytetrahydrofuran diol is 500-2000.

4. A modified waterproof coating according to claim 3, characterized in that: The fluorine-containing compound is perfluorooctyl phosphate or perfluorooctyl ethanol; The fluorine content of the fluorine-containing compound is greater than 60%, and the molecular weight is 400-600.

5. The modified waterproof coating according to claim 3, characterized in that: The nano inorganic material is nano silicon dioxide and / or nano zinc oxide.

6. A modified waterproof coating according to claim 3, characterized in that: The antioxidant is any one of TINUVIN 144, TINUVIN 622, BHT and BHA.

7. The modified waterproof coating according to claim 3, characterized in that: The plasticizer is dioctyl phthalate, the filler is silicon dioxide, and the defoamer is TEGO Foamex K3.

8. A method for preparing the modified waterproof coating according to any one of claims 1 to 7, characterized in that: The following steps are involved: Mix hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate with polypropylene glycol and polytetramethylene glycol, and react at 60-80°C for 4-8h. When the conversion rate of the active groups of hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate is at least 80% or the reaction time is reached, terminate the reaction to obtain an isocyanate prepolymer; Adding the nano inorganic material into ethanol or xylene and dispersing it using a high shear mixer; In a reaction kettle, the isocyanate prepolymer, the fluorine-containing compound, the nano inorganic material, and a plasticizer, a filler and a defoamer are added in sequence, and the stirring speed is maintained at 300-500 rpm for 30 minutes; Gradually add antioxidants, and continue stirring at a stirring speed of 300-500 rpm for 10-15 minutes; after standing for 2-4 hours, filter through an 80-mesh sieve to remove large solid particles to obtain a modified waterproof coating.

9. The method for preparing the modified waterproof coating according to claim 8, characterized in that: When preparing the isocyanate prepolymer, the added mass ratio of hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate to polypropylene glycol diacid or polytetramethylene glycol is 1:1.2-1.

5.

10. The method for preparing the modified waterproof coating according to claim 9, characterized in that: The high shear mixer is set to have a rotation speed of 1000-5000 RPM, a feed rate of 1-5 kg / min, and a dispersion time of 30-60 min.

Citation Information

Patent Citations

  • Method for preparing high-performance single-component polyurethane waterproof coating

    CN101987940A

  • One-component self-curing polyurethane waterproof coating

    CN102504690A

  • Vehicle paint and production method thereof

    CN109096884A

  • Environment-friendly single-component polyurethane waterproof coating

    CN111117465A

  • Odorless polyurethane waterproof coating and preparation method thereof

    CN111592821A