Composition and application thereof
Through the composition of specific structurally modified particles, the removal rate of silicon nitride is improved by using electrostatic attraction and chemical corrosion, which solves the problems of slow silicon nitride removal rate and high defect value in electronic product manufacturing, and achieves efficient surface flatness .
Patent Information
- Application Number
- CN202310623934.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
During the manufacturing process of electronic products, the removal rate of silicon nitride is slow and the defect value on the substrate surface after grinding is high. Traditional silicon sols and commercial sulfonic acid modified silicon dioxide have insufficient mechanical effects and high defects during the grinding process. .
Provided is a composition including modified particles, pH adjusters and solvents that modify oxide particles through negatively charged modified groups of specific structures, increase the removal rate of silicon nitride by electrostatic attraction and chemical corrosion, and Reduce surface defects.
The removal rate and flattening effect of silicon nitride are significantly improved, residual particles on the surface after grinding are reduced, and a lower defect value is obtained, and the grinding efficiency and quality are improved.
Smart Images

Figure CN119060635A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the technical field of electronic product manufacturing, and in particular, to a composition and its application. Background Art
[0002] In the manufacturing process of electronic products, it is usually involved in the surface treatment process of grinding metals, silicon, silicon oxide, polysilicon, silicon nitride and other materials. This process needs to control the removal rate of each material according to the structure of the product. Among them, silicon nitride (SiN) has a high hardness. When it is ground using traditional silica sol, the mechanical action between the silica sol and the grinding layer is weak, which makes the removal rate of SiN slow; and when using the currently commercial sulfonic acid-modified silica, although the removal rate of SiN is improved compared with traditional silica sol, the defect value of the substrate surface after grinding is higher. In order to better meet the process requirements, it is necessary to provide a new abrasive to increase the removal rate of SiN and obtain a lower defect value. Summary of the invention
[0003] In view of this, an embodiment of the present application provides a composition, which includes oxide particles modified by special structural groups. The composition can be used for grinding various semiconductor substrates, especially for grinding silicon nitride, to increase the removal rate of silicon nitride and obtain a lower defect value.
[0004] Specifically, the first aspect of the embodiment of the present application provides a composition, the composition comprising modified particles, a pH adjuster and a solvent, the modified particles comprising oxide particles and a modifying group represented by formula (1) bonded to the oxide particles;
[0005]
[0006] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0007] The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
[0008] The composition of the embodiment of the present application can be used for surface flattening of semiconductor substrates in the process of preparing electronic products, that is, the composition of the embodiment of the present application is a liquid flattening composition, which uses modified oxide particles as abrasives, wherein the modified oxide particles are obtained by modifying the oxide particles through the negatively charged modified groups of the structure shown in formula (1). The modified oxide particles can generate a strong electrostatic attraction between their negative charge and the semiconductor substrate to be processed with a positive charge on the surface, thereby facilitating the mechanical grinding effect; at the same time, the negatively charged modified groups of the structure shown in formula (1) can be used as nucleophilic agents to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of chemical bonds; the above two effects can greatly improve the removal rate of the semiconductor substrate material. The composition can be used for surface flattening of various semiconductor substrates in the process of preparing electronic products, and can be used in particular for grinding semiconductor substrates with positive charges on the surface, and improving the removal rate of semiconductor substrate materials with positive charges on the surface, for example, it can be used for grinding silicon nitride, and improving the removal rate of silicon nitride. In addition, since the negatively charged modified group of the structure shown in formula (1) of the present application has a lower degree of ionization, there are fewer residual particles on the surface of the semiconductor substrate after grinding, which is easier to clean, resulting in a lower defect value and improved flattening effect.
[0009] In the embodiment of the present application, the content of X atoms in the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 0.01 atomic % (atomic percentage) and less than or equal to 30 atomic %. That is, the atomic percentage of X atoms in the modified particles characterized by the X-ray photoelectron spectrometer is 0.01%-30%. The X atoms are derived from the modifying groups, and the appropriate amount of X atoms indicates that an appropriate amount of modifying groups are bound to the surface of the oxide particles. In the embodiment of the present application, by controlling the atomic percentage of X atoms on the surface of the modified particles within a suitable range, a better modification effect can be obtained, thereby improving the removal rate of the semiconductor substrate material by the composition.
[0010] In the embodiment of the present application, the carbon atom content of the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 2 atomic % and less than or equal to 45 atomic %. That is, the atomic percentage of carbon atoms of the modified particles characterized by the X-ray photoelectron spectrometer is 2%-45%. Carbon atoms come from the modifying groups, and the appropriate carbon atom content can reflect the modification amount of the modifying groups. In the embodiment of the present application, by controlling the atomic percentage of carbon atoms on the surface of the modified particles within a suitable range, a better modification effect can be obtained, thereby improving the removal rate of the semiconductor substrate material by the composition.
[0011] In the embodiment of the present application, the oxide particles are silicon dioxide particles, and the ratio of the number of X atoms to the number of silanol groups of the modified particles is greater than or equal to 0.4% and less than or equal to 48%. The ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles can reflect the relationship between the number of modified groups and the number of remaining silanol groups on the surface of the silicon dioxide particles after modification. In the embodiment of the present application, by controlling the ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles within a suitable range, a better modification effect can be obtained, thereby improving the removal rate and / or selectivity of the composition for semiconductor substrate materials with positive surface charge.
[0012] The ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles can be characterized and calculated as follows:
[0013] The X element content of the modified particles is characterized by inductively coupled plasma emission spectroscopy (ICP), and the number of X atoms per unit weight of the modified particles is obtained by conversion. The number of silanol groups per unit weight of the modified particles can be determined by using commonly used published titration methods (such as acid-base titration, potentiometric titration, etc.). The number of X atoms per unit weight of the modified particles is divided by the number of silanol groups per unit weight of the modified particles to obtain the ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles.
[0014] In the embodiment of the present application, the modified group is bonded to the oxide particle by chemical bonding. The modified group is bonded to the surface of the oxide particle by chemical bonding, so that the modified group with specific properties can be stably present on the surface of the oxide particle, so that the modified particle can achieve a uniform and stable flattening effect when treating the surface of the semiconductor substrate. The chemical bonding can be covalent bonding.
[0015] In the implementation mode of the present application, the average particle size of the modified particles measured by dynamic light scattering (DLS) is 5nm-500nm (i.e., greater than or equal to 5nm and less than or equal to 500nm). The average particle size measured by the dynamic light scattering method can be understood as the average particle size of the secondary particles formed by the agglomeration or association of the primary particles. In one embodiment of the present application, the modified particles are modified silica particles, and the modified particles are modified colloidal silica. The modified particles have a smaller particle size, which is beneficial to reduce the generation of scratches on the surface of the semiconductor substrate (such as a semiconductor substrate) during the grinding process and improve the grinding quality. In some embodiments of the present application, the average particle size of the modified particles is 10nm-300nm. In some embodiments of the present application, the average particle size of the modified particles is 20nm-200nm. In some embodiments of the present application, the average particle size of the modified particles is 25nm-100nm. The modified particles have a suitable particle size, which can better take into account the problem of flattening rate and surface scratches.
[0016] In the embodiment of the present application, the weight proportion of the modified particles in the composition is 0.1%-50%. The modified particles, as abrasives, have a direct impact on the flattening effect. The appropriate amount of modified particles in the composition is conducive to generating sufficient chemical corrosion and mechanical friction to jointly achieve efficient removal of the semiconductor substrate, while maintaining the composition with suitable fluidity and maintaining high uniformity of the modified particles in the composition.
[0017] In the embodiment of the present application, the pH of the composition is less than 12. The pH of the composition of the present application can be adjusted by a pH adjuster, and the pH of the composition can be controlled at a suitable value, which is beneficial to improve the removal rate of the semiconductor substrate.
[0018] In some embodiments of the present application, the pH of the composition is 1-6. Since the composition of the present application uses oxide particles modified by the modifying group of the structure shown in formula (1) as abrasives, and in practical applications, most semiconductor substrate surfaces are positively charged, considering that the use of a negatively charged planarization composition can better promote the removal rate of positively charged semiconductor substrates, controlling the pH of the composition to 1-6 is beneficial to improving the removal rate of positively charged semiconductor substrates.
[0019] In the embodiment of the present application, the average degree of association of the modified particles is 1-10 (i.e., greater than or equal to 1 and less than or equal to 10). The average degree of association is the average particle size (nm) of the modified particles / the average primary particle size (nm) of the modified particles. The value of the average primary particle size can be calculated based on the specific surface area of the modified particles measured by the BET method, and the average particle size is measured by the dynamic light scattering method. In the embodiment of the present application, the average degree of association of the modified particles is controlled at 1-10, which can better avoid the influence of the modified particles on the flattening effect due to the dispersion problem.
[0020] In the embodiment of the present application, the potential of the composition is in the range of -55 to -5. The potential here refers to the overall potential of the composition, and the potential value of the composition can be obtained by measuring the potential value of the composition using a Zeta potential meter according to an electrophoretic light scattering method. By controlling the overall potential of the composition within the above range, the influence of the potential factor on the planarization effect can be better avoided.
[0021] In the embodiment of the present application, the substituted or unsubstituted alkyl group is a substituted or unsubstituted C1-C6 alkyl group, the substituted or unsubstituted alkoxy group is a substituted or unsubstituted C1-C6 alkoxy group; the substituted or unsubstituted alkylene group is a substituted or unsubstituted C1-C6 alkylene group, and the substituted or unsubstituted alkyleneoxy group is a substituted or unsubstituted C1-C6 alkyleneoxy group. Controlling the carbon chain length of the substituted or unsubstituted alkylene group, substituted or unsubstituted alkoxy group, substituted or unsubstituted alkylene group, and substituted or unsubstituted alkyleneoxy group in the modifying group within a suitable range is beneficial to controlling the hydrophilic and hydrophobic properties of the modifying group on the one hand, so that the modified particles can better grind the semiconductor substrate; on the other hand, it is beneficial for the modifying group to better modify the silica particles and avoid the adverse effects caused by the excessive volume steric hindrance of the modifying group.
[0022] In the embodiment of the present application, the pH regulator includes an acid, or a composition formed by an acid and a base or a base salt, and the acid includes an organic acid and / or an inorganic acid. The pH regulator has the function of adjusting the pH of the composition. In some embodiments, the pH regulator may include only one or more organic acids; in some embodiments, the pH regulator may include only one or more inorganic acids; in some embodiments, the pH regulator may include both one or more organic acids and one or more inorganic acids. In some embodiments, the pH regulator may also use the above-mentioned one or more acids in combination with one or more bases or base salts. In the combination of acid and base or base salt, the effect of simultaneously adjusting pH and conductivity can be achieved.
[0023] Among them, organic acid can be various monocarboxylic acids, dicarboxylic acids, tricarboxylic acids, such as but not limited to formic acid, acetic acid, propionic acid, butyric acid, 2-methylbutyric acid, 2-ethylbutyric acid, 3,3-dimethylbutyric acid, valeric acid, 4-methylvaleric acid, n-hexanoic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, n-heptanoic acid, n-octanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, phthalic acid, malic acid, tartaric acid, citric acid, maleic acid, lactic acid, diglycolic acid. Inorganic acid, such as but not limited to hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid and phosphoric acid. Alkali can be amines such as quaternary ammonium hydroxide, aliphatic amines, aromatic amines, alkali metal hydroxides, alkaline earth metal hydroxides, and ammonia. Alkali salts can use ammonium salts and alkali metal salts of the aforementioned acids.
[0024] It is understood that in order to increase the removal rate of the composition from the semiconductor substrate, the pH adjuster can be an acid selected to be beneficial to increasing the removal rate of the semiconductor substrate, or a combination of an acid and a base or a base salt.
[0025] In the embodiment of the present application, the solvent may include water or an organic solvent. Water and organic solvents serve as dispersion media for the modified particles and other components of the composition in the composition, wherein the organic solvent may be any organic solvent that is conducive to the dispersion of the modified particles and other components of the composition.
[0026] In the embodiments of the present application, in order to improve certain aspects of the performance of the composition and better meet the surface planarization treatment of semiconductor substrates in various scenarios, the composition may also include other additives, which may be but are not limited to one or more of catalysts, oxidants, surfactants, preservatives, passivators, and reducing agents.
[0027] In the embodiment of the present application, the mass content of the solvent in the composition is greater than or equal to 50% and less than 100%. The composition with a larger mass content of solvent can have better fluidity, which is beneficial for the particles in the composition to maintain good dispersion and can also control the grinding effect of the composition on the semiconductor substrate.
[0028] In the embodiment of the present application, the viscosity of the composition at 25° C. is 1-80 centipoise (cP). The composition has a suitable room temperature viscosity, which is conducive to its faster and uniform spreading during the leveling process, and is conducive to the full fluidity of the particles in the composition, improving the grinding efficiency, and obtaining a better grinding effect.
[0029] In the embodiment of the present application, the removal rate of silicon nitride by the composition is greater than The composition of the embodiment of the present application can achieve high-speed removal of silicon nitride by adding modified particles with a specific structure and utilizing the strong chemical action and mechanical grinding action of the modified particles on silicon nitride, thereby improving the grinding efficiency.
[0030] In the embodiment of the present application, the removal selectivity of the composition for silicon nitride and silicon oxide is greater than 1.5. The composition of the embodiment of the present application has a high removal selectivity for silicon nitride and silicon oxide, and can preferably remove silicon nitride preferentially when performing surface planarization treatment on a semiconductor substrate containing both silicon nitride and silicon oxide on the surface.
[0031] The second aspect of the embodiment of the present application provides the use of the composition described in the first aspect in surface treatment of a semiconductor substrate. The surface treatment is specifically surface flattening treatment, and the composition is used as a polishing liquid.
[0032] In the embodiment of the present application, the application may specifically be to use the composition to perform surface planarization treatment on a semiconductor substrate with a positively charged surface. The use of the composition of the embodiment of the present application may increase the removal rate of the semiconductor substrate material with a positively charged surface.
[0033] In the embodiment of the present application, the application is to use the composition to perform surface treatment on semiconductors containing nitrogen-silicon bonds on the surface. For example, it can be used for grinding silicon nitride to increase the removal rate of silicon nitride. On the one hand, the modified particles in the embodiment of the present application composition can utilize their negative charge to generate a strong electrostatic attraction between the surface of the semiconductor substrate to be treated with positive charge, which is conducive to enhancing the mechanical grinding effect; at the same time, the negatively charged modified group can be used as a nucleophilic agent to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of the chemical bonds; the above two aspects can greatly increase the removal rate of the semiconductor substrate material.
[0034] The third aspect of the embodiment of the present application provides a surface treatment method, wherein the composition described in the first aspect contacts and grinds the surface of the semiconductor substrate to be treated. The surface treatment method uses the composition as a grinding liquid to grind the surface of the semiconductor substrate to be treated. The surface treatment method uses the composition of the embodiment of the present application to improve the treatment efficiency and treatment effect.
[0035] The embodiment of the present application also provides a modified particle dispersion for surface treatment of a semiconductor substrate, wherein the modified particle dispersion comprises modified particles and a solvent, wherein the modified particles comprise oxide particles and a modified group represented by formula (1) bonded to the oxide particles;
[0036]
[0037] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0038] The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
[0039] The modified particle dispersion of the embodiment of the present application can be used as an abrasive raw material to prepare a planarizing composition for surface planarizing treatment of a semiconductor substrate. The modified particles in the modified particle dispersion are modified with negatively charged modified groups of a special structure, and can be used for grinding semiconductor substrates with positively charged surfaces, thereby increasing the removal rate of semiconductor substrate materials with positively charged surfaces, and can also enable the semiconductor substrate to obtain a lower defect value after surface planarization treatment.
[0040] The embodiment of the present application also provides a semiconductor substrate, which is obtained by subjecting the surface of the semiconductor substrate to a planarization treatment using the composition described in the first aspect of the embodiment of the present application.
[0041] In an embodiment of the present application, the semiconductor substrate includes silicon nitride and / or silicon oxide.
[0042] An embodiment of the present application also provides a semiconductor device, comprising the semiconductor substrate described above in the embodiment of the present application, and a functional layer disposed on the semiconductor substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a schematic diagram of the process operation of chemical-mechanical polishing in the application scenario of this application;
[0044] Figure 2 is a schematic structural diagram of a modified particle 10 according to an embodiment of the present application;
[0045] Figure 3 FIG. 1 is a schematic structural diagram of a semiconductor device 100 according to an embodiment of the present application. DETAILED DESCRIPTION
[0046] The embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application.
[0047] The application scenario involved in this application is chemical-mechanical polishing. Chemical-mechanical polishing refers to the process in which, under certain pressure and the presence of abrasive liquid, abrasive liquid containing abrasives chemically corrodes the abrasive layer, while the abrasives grind the abrasive layer mechanically, and the abrasive layer gradually becomes flat. Figure 1 As shown, during the chemical-mechanical polishing process, the semiconductor substrate 103 is fixed at the bottom of the grinding head 104, and the rotating grinding head 104 is pressed on the rotating grinding pad 102 located on the grinding table 101 with a certain pressure, and the grinding liquid 105 flows between the surface of the semiconductor substrate 103 and the grinding pad 102, and is evenly distributed into a liquid film under the transmission and centrifugal action of the grinding pad 102. Through the dual chemical and mechanical effects of the liquid, the surface of the semiconductor substrate is smoothed and made highly flat.
[0048] In the process of manufacturing electronic products, it is usually involved in the surface treatment process of grinding materials such as metals, silicon, silicon oxide, polysilicon, silicon nitride, etc. This process needs to control the removal rate of each material according to the structure of the product. Among them, silicon nitride (SiN) has a high hardness. When it is ground using traditional silica sol, the mechanical action between the silica sol and the grinding layer is weak, which makes the removal rate of SiN slow; and the use of currently commercial sulfonic acid-modified silicon dioxide, although the removal rate of SiN is improved compared with traditional silica sol, the defect value of the substrate surface after grinding is higher. In order to better meet the process requirements, the embodiment of the present application provides a composition, which can be used as a grinding liquid for grinding various semiconductor substrates, especially for grinding silicon nitride, to improve the removal rate of silicon nitride and obtain a lower defect value.
[0049] Specifically, the present invention provides a composition comprising modified particles, a pH regulator and a solvent, wherein: Figure 2 As shown, the modified particle 10 includes an oxide particle 11 and a modified group 12 represented by formula (1) bonded to the oxide particle 11;
[0050]
[0051] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0052] The oxide particles 11 include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
[0053] The composition of the embodiment of the present application can be used for surface flattening of semiconductor substrates in the process of preparing electronic products, that is, the composition of the embodiment of the present application is a liquid flattening composition, which uses modified oxide particles as abrasives, wherein the modified oxide particles are obtained by modifying the oxide particles through the negatively charged modified groups of the structure shown in formula (1). The modified oxide particles can generate a strong electrostatic attraction between their negative charge and the semiconductor substrate to be processed with a positive charge on the surface, thereby facilitating the mechanical grinding effect; at the same time, the negatively charged modified groups of the structure shown in formula (1) can be used as nucleophilic agents to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of chemical bonds; the above two effects can greatly improve the removal rate of the semiconductor substrate material. The composition can be used for surface flattening of various semiconductor substrates in the process of preparing electronic products, and can be used in particular for grinding semiconductor substrates with positive charges on the surface, and improving the removal rate of semiconductor substrate materials with positive charges on the surface, for example, it can be used for grinding silicon nitride, and improving the removal rate of silicon nitride. In addition, since the negatively charged modified group of the structure shown in formula (1) of the present application has a lower degree of ionization, there are fewer residual particles on the surface of the semiconductor substrate after grinding, which is easier to clean, resulting in a lower defect value and improved flattening effect.
[0054] In the embodiment of the present application, the content of X atoms in the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 0.01 atomic % and less than or equal to 30 atomic %. That is, the atomic percentage of X atoms in the modified particles characterized by the X-ray photoelectron spectrometer is 0.01%-30%. The X atoms are derived from the modifying groups, and the appropriate amount of X atoms indicates that an appropriate amount of modifying groups are bound to the surface of the oxide particles. The embodiment of the present application controls the atomic percentage of X atoms on the surface of the modified particles within a suitable range, and can obtain a better modification effect. It can also regulate the hydrophilicity / hydrophobicity of the modified particles, thereby regulating the effective contact area of the composition to the semiconductor substrate material, and regulating the removal rate of the composition to the semiconductor substrate material. Exemplarily, the content of X atoms in the modified particles measured by X-ray photoelectron spectroscopy is 0.05 atomic %, 0.1 atomic %, 0.5 atomic %, 1 atomic %, 2 atomic %, 5 atomic %, 10 atomic %, 15 atomic %, 20 atomic %, 25 atomic %, 30 atomic %.
[0055] In the embodiment of the present application, the content of carbon atoms in the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 2 atomic % and less than or equal to 45 atomic %. That is, the atomic percentage of carbon atoms in the modified particles characterized by the X-ray photoelectron spectrometer is 2%-45%. Carbon atoms come from the modifying group, and the appropriate amount of carbon atom content can reflect the modification amount of the modifying group. The embodiment of the present application controls the atomic percentage of carbon atoms on the surface of the modified particles within a suitable range, and can obtain a better modification effect. It can also regulate the hydrophilicity / hydrophobicity of the modified particles, thereby regulating the effective contact area of the composition to the semiconductor substrate material and improving the removal rate of the composition to the semiconductor substrate material. Exemplarily, the content of carbon atoms in the modified particles measured by X-ray photoelectron spectroscopy is 2 atomic %, 5 atomic %, 10 atomic %, 15 atomic %, 20 atomic %, 25 atomic %, 30 atomic %, 35 atomic %, 40 atomic %, 45 atomic %.
[0056] In some embodiments of the present application, the oxide particles are silicon dioxide particles, and the ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups (Si-OH) is greater than or equal to 0.4% and less than or equal to 48%. The ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups can reflect the relationship between the number of modified groups on the surface of the silicon dioxide particles after modification and the number of remaining silanol groups. The embodiments of the present application can obtain a better modification effect by controlling the ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups within a suitable range, thereby improving the removal rate and / or selectivity of the composition for semiconductor substrate materials with positive surface charge. Exemplarily, the ratio of the number of X atoms on the surface of the modified particles to the number of silanol groups can be 0.5%, 5%, 8%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 46%, 47%, 48%.
[0057] The ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles can be characterized and calculated as follows:
[0058] The X element content of the modified particles is characterized by inductively coupled plasma emission spectroscopy (ICP), and the number of X atoms per unit weight of the modified particles is obtained by conversion. The number of silanol groups per unit weight of the modified particles can be determined by using commonly used published titration methods (such as acid-base titration, potentiometric titration, etc.). The number of X atoms per unit weight of the modified particles is divided by the number of silanol groups per unit weight of the modified particles to obtain the ratio of the number of X atoms to the number of silanol groups on the surface of the modified particles.
[0059] In the embodiment of the present application, the modified group 12 is chemically bonded to the surface of the oxide particle 11, so that the modified group with specific properties can be stably present on the surface of the oxide particle, so that the modified particle can achieve a uniform and stable flattening effect when treating the surface of the semiconductor substrate, and obtain a better flattening effect. The chemical bonding can be covalent bonding. For example, the modified group can form a covalent bond with the silanol group on the surface of the silica particle through the R3 group.
[0060] In the implementation mode of the present application, the average particle size of the modified particles measured by a dynamic light scattering instrument according to the dynamic light scattering method (Dynamic Light Scattering, DLS) is 5nm-500nm (i.e. greater than or equal to 5nm and less than or equal to 500nm). The average particle size measured by the dynamic light scattering method can be understood as the average particle size of the secondary particles formed by the agglomeration or association of the primary particles. The average particle size of the modified particles is less than or equal to 500nm. In the embodiment of the present application, the modified particles are modified silica particles, specifically modified colloidal silica. The modified particles have a smaller particle size, which is beneficial to reduce the generation of scratches on the surface of the semiconductor substrate during the grinding process and improve the grinding quality. In some embodiments of the present application, the average particle size of the modified particles is 10nm-300nm. In some embodiments, the average particle size of the modified particles is 20nm-200nm. In some embodiments, the average particle size of the modified particles is 25nm-100nm. The modified particles have a suitable particle size, which can better take into account the flattening rate and surface scratches. Illustratively, the average particle size of the modified particles can be 5 nm, 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 120 nm, 150 nm, 200 nm, 250 nm, 300 nm, 400 nm, or 500 nm.
[0061] In the embodiment of the present application, in the composition, the weight proportion of the modified particles is 0.1%-50%. As an abrasive, the modified particles have a direct impact on the flattening effect. The appropriate amount of modified particles in the composition is conducive to producing sufficient chemical corrosion and mechanical friction to jointly achieve efficient removal of semiconductor substrate materials, while keeping the composition suitable for fluidity and maintaining high uniform dispersion of the modified particles in the composition. Exemplarily, the weight proportion of the modified particles in the composition is 0.1%, 0.5%, 1%, 3%, 5%, 8%, 10%, 20%, 25%, 30%, 35%, 40%, 45%, 50%. The composition is centrifuged to remove the supernatant, and the solid content is obtained after the remaining part of the precipitate is dried to obtain the weight proportion of the modified particles.
[0062] In the embodiment of the present application, the pH of the composition is less than 12. The composition of the present application can adjust the pH by a pH adjusting agent, and the pH of the composition is controlled at a suitable value, which is conducive to improving the removal rate of the semiconductor substrate material. In the present application, the pH of the composition can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, for example.
[0063] In some embodiments of the present application, the pH of the composition is 1-6. Since the composition of the present application uses oxide particles modified with a modifying group having a structure shown in formula (1) as an abrasive, and in actual applications, many semiconductor substrate surfaces are positively charged, and considering that the use of a negatively charged planarization composition can better promote the removal rate of positively charged semiconductor substrates, controlling the pH of the composition to 1-6 is beneficial to improving the removal rate of positively charged semiconductor substrates.
[0064] In the embodiment of the present application, the average degree of association of the modified particles is 1-10 (i.e., greater than or equal to 1 and less than or equal to 10). The average degree of association is the average particle size (nm) of the modified particles / the average primary particle size (nm) of the modified particles. The value of the average primary particle size can be calculated based on the specific surface area of the modified particles measured by the BET method, and the average particle size is measured by a dynamic light scattering method. In the embodiment of the present application, the average degree of association of the modified particles is controlled at 1-10, which can better avoid the influence of the modified particles on the flattening effect due to the dispersion problem. Exemplarily, the average degree of association of the modified particles can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10.
[0065] In the embodiment of the present application, the potential of the composition is in the range of -55 to -5. Here, the potential is the overall potential of the composition, and a Zeta potential meter can be used to measure the potential value of the composition according to the electrophoretic light scattering method. By controlling the overall potential of the composition within the above range, the influence of the potential factor on the flattening effect can be better avoided. Exemplarily, the potential of the composition can be -55, -50, -40, -35, -30, -25, -20, -15, -10, -5.
[0066] In the embodiment of the present application, in the modified group of the structure shown in formula (1), the substituted or unsubstituted alkyl is a substituted or unsubstituted C1-C6 alkyl, the substituted or unsubstituted alkoxy is a substituted or unsubstituted C1-C6 alkoxy; the substituted or unsubstituted alkylene is a substituted or unsubstituted C1-C6 alkylene, and the substituted or unsubstituted alkyleneoxy is a substituted or unsubstituted C1-C6 alkyleneoxy. Controlling the carbon chain length of the substituted or unsubstituted alkylene, substituted or unsubstituted alkoxy, substituted or unsubstituted alkylene, and substituted or unsubstituted alkyleneoxy in the modified group within a suitable range is beneficial to controlling the hydrophilic and hydrophobic properties of the modified group on the one hand, so that the modified particles can better grind the semiconductor substrate; on the other hand, it is beneficial for the modified group to better modify the silica particles and avoid the adverse effects caused by the excessive volume steric hindrance of the modified group. For example, substituted or unsubstituted C1-C6 alkyl can be substituted or unsubstituted methyl (-CH3), substituted or unsubstituted ethyl (-CH2CH3), substituted or unsubstituted propyl group, substituted or unsubstituted butyl, substituted or unsubstituted pentyl, substituted or unsubstituted hexyl.Substituted or unsubstituted C1-C6 alkoxy can be substituted or unsubstituted methoxy (-OCH3), substituted or unsubstituted ethoxy (-OCH2CH3), substituted or unsubstituted propoxy, substituted or unsubstituted butoxy, substituted or unsubstituted pentyloxy, substituted or unsubstituted hexyloxy.Substituted or unsubstituted C1-C6 alkylene can be substituted or unsubstituted methylene (-CH2-), substituted or unsubstituted ethylidene (-CH2CH2-), substituted or unsubstituted propylene, substituted or unsubstituted butylene, substituted or unsubstituted pentylene, substituted or unsubstituted hexylene. Substituted or unsubstituted C1-C6 alkyleneoxy may be substituted or unsubstituted methyleneoxy (-OCH2-), substituted or unsubstituted ethyleneoxy (-OCH2CH2-), substituted or unsubstituted propyleneoxy, substituted or unsubstituted butyleneoxy, substituted or unsubstituted pentyleneoxy, substituted or unsubstituted hexyleneoxy. Substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy may be a straight chain structure or a straight chain structure. Among them, the substituent groups in the substituted alkyl, substituted alkoxy, substituted alkylene and substituted alkyleneoxy may be halogen atoms, alkyl, aryl, amino, alkali metal elements, etc.
[0067] In the embodiment of the present application, the pH regulator is an acid, or a composition formed by an acid and a base or a base salt, and the acid includes an organic acid and / or an inorganic acid. In some embodiments, the pH regulator may include only one or more organic acids; in some embodiments, the pH regulator may include only one or more inorganic acids; in some embodiments, the pH regulator may include both one or more organic acids and one or more inorganic acids. In some embodiments, the pH regulator may also be used in combination with one or more of the above-mentioned acids and one or more bases or base salts. In the combination of acid and base or base salt, the effect of simultaneously adjusting pH and conductivity can be achieved.
[0068] Among them, the organic acid can be various monocarboxylic acids, dicarboxylic acids, tricarboxylic acids, and specific examples include but are not limited to formic acid, acetic acid, propionic acid, butyric acid, 2-methylbutyric acid, 2-ethylbutyric acid, 3,3-dimethylbutyric acid, valeric acid, 4-methylvaleric acid, n-hexanoic acid, 2-methylhexanoic acid, 2-ethylhexanoic acid, n-heptanoic acid, n-octanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, phthalic acid, malic acid, tartaric acid, citric acid, maleic acid, lactic acid, and diglycolic acid. Inorganic acids include but are not limited to hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid.
[0069] It is understandable that in order to increase the removal rate of the composition to the semiconductor substrate, the pH adjuster can be an acid selected to be beneficial to increase the removal rate of the semiconductor substrate, or a combination of an acid and a base or a base salt. The acid can be an acid containing a carboxylate, a phosphonate, or a phosphate.
[0070] The modified particles of the embodiments of the present application can adapt to a variety of organic acids and inorganic acids as the composition system of the pH adjuster, and can effectively improve the removal rate of semiconductor substrate materials such as silicon nitride in different pH adjuster systems.
[0071] In the embodiment of the present application, the solvent may include water or an organic solvent. Water and organic solvents serve as dispersion media for the modified particles and other components of the composition in the composition, wherein the organic solvent may be various organic solvents that are conducive to the dispersion of the modified particles and other components of the composition, for example, the organic solvent may be ethanol, methanol, isopropanol, n-butanol, acetone, butanone, dimethyl carbonate, etc.
[0072] In the embodiment of the present application, in order to improve the performance of certain aspects of the composition, better meet the surface flattening treatment of semiconductor substrates in various scenarios, the composition may also include other additives, other additives may be but not limited to catalysts, oxidants, surfactants, preservatives, passivators, reducing agents, one or more. For example, the oxidant may be one or more of hydrogen peroxide, ammonium persulfate, periodic acid, hypochlorous acid, etc., for promoting oxidation of the surface of the grinding object, regulating its removal rate. The preservative may be isothiazolinone and other isothiazolinone system preservatives, parabens, and phenoxyethanol, etc., these preservatives can be used alone or in combination. Adding a preservative is used to extend the service life of the composition, which plays a role in inhibiting deterioration. The surfactant may be a water-soluble polymer such as cellulose, polyvinyl pyrrolidone, polyethyleneimine, polyacrylic acid, polyvinyl alcohol, etc., and the surfactant plays a role in improving the stability of the particles, or regulating the interaction between the particles and the grinding object to regulate the removal rate.
[0073] The preparation method of the composition of the embodiment of the present application can be: adding a solvent to the modified colloidal silica, then adding a pH adjuster, and fully mixing under stirring conditions to obtain the composition. The pH of the composition is adjusted to a desired value by controlling the amount of the pH adjuster added.
[0074] The present application does not particularly limit the method for modifying the surface of oxide particles with the modifying group shown in formula (1). For example, the modified particles can be obtained by heating and stirring the raw oxide particles with one or more modifiers containing the modifying group of formula (1) or more under solvent conditions, so that the modifying group of formula (1) is bound to the surface of the oxide particles to obtain oxide particles modified with the structural modifying group of formula (1). The modified particles can also be obtained by first reacting the modifying group of formula (1) with a protective group to the surface of the oxide particles, and then adding a reagent for removing the protective group to remove the protective group after the reaction is completed, and finally obtaining oxide particles modified with the structural modifying group of formula (1). The solvent can be an aqueous medium or an organic medium. The aqueous medium can be water or a combination of water and one or more water-soluble solvents such as methanol, ethanol, isopropanol, acetone, butanone, etc. The organic medium can be one or more combination of conventional organic solvents such as methanol, ethanol, isopropanol, acetone, butanone, toluene, xylene, ethyl acetate, dimethyl carbonate, etc.
[0075] In the embodiment of the present application, the mass content of the solvent in the composition is greater than or equal to 50% and less than 100%. The composition has a larger amount of solvent to have better fluidity and can also control the grinding effect of the composition on the semiconductor substrate. Exemplarily, the mass content of the solvent in the composition can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%.
[0076] In the embodiment of the present application, the viscosity of the composition at 25°C is 1 centipoise to 80 centipoise (cP). The composition has a suitable room temperature viscosity, which is conducive to its faster and uniform development during the leveling process, improves the grinding efficiency, and obtains a better grinding effect. Exemplarily, the viscosity of the composition at 25°C is 1 centipoise, 5 centipoise, 10 centipoise, 25 centipoise, 30 centipoise, 40 centipoise, 50 centipoise, 60 centipoise, 65 centipoise, 80 centipoise (cP).
[0077] In the embodiment of the present application, the removal rate of the composition for silicon nitride is greater than The composition of the present application embodiment adds modified particles with a specific structure as abrasives, and utilizes the strong chemical action and mechanical grinding action of the modified particles on silicon nitride to achieve high-speed removal of silicon nitride, thereby improving the grinding efficiency. In some embodiments, the removal rate of silicon nitride by the composition is greater than In some embodiments, the composition has a removal rate of silicon nitride greater than In some embodiments, the composition has a removal rate of silicon nitride greater than In some embodiments, the composition has a removal rate of silicon nitride greater than In some embodiments, the composition has a removal rate of silicon nitride greater than In some embodiments, the composition has a removal rate of silicon nitride greater than
[0078] In the embodiment of the present application, the removal selectivity of the composition for silicon nitride and silicon oxide is greater than 1.5. The composition of the embodiment of the present application has a higher removal selectivity of silicon nitride and silicon oxide, and can preferably remove silicon nitride preferentially when the surface of a semiconductor substrate containing both silicon nitride and silicon oxide is subjected to surface planarization treatment. In some embodiments, the removal selectivity of the composition for silicon nitride and silicon oxide is greater than 2. In some embodiments, the removal selectivity of the composition for silicon nitride and silicon oxide is greater than 3. In some embodiments, the removal selectivity of the composition for silicon nitride and silicon oxide is greater than 5. In some embodiments, the removal selectivity of the composition for silicon nitride and silicon oxide is greater than 10. In some embodiments, the removal selectivity of the composition for silicon nitride and silicon oxide is greater than 15.
[0079] In the embodiment of the present application, after the semiconductor substrate is surface treated with the composition of the embodiment of the present application, under the same conditions, a relatively lower defect value can be obtained than that of the planarization composition using commercial sulfonic acid group-modified silica as an abrasive.
[0080] The embodiments of the present application also provide the application of the above-mentioned composition in the surface treatment of semiconductor substrates. The surface treatment is specifically a surface flattening treatment, and the composition is used as a polishing liquid. The application of the present application can specifically be to use the composition to perform surface flattening treatment on a semiconductor substrate with a positively charged surface. The use of the composition of the embodiments of the present application can increase the removal rate of semiconductor substrate materials with a positively charged surface. And because the negatively charged modified group of the structure shown in formula (1) of the present application has a relatively high PKa value compared with the common organic acid sulfonic acid group or the strong acidic group nitrate and sulfate, it can be understood that under the same low pH conditions, the group shown in structural formula (1) has a relatively low degree of dissociation, which can reduce the residual particles on the surface of the semiconductor substrate after grinding, make it easier to clean, obtain a lower defect value, and improve the flattening effect.
[0081] The semiconductor substrate of the embodiment of the present application may be a substrate to be planarized produced at various process nodes in the process of manufacturing electronic products, for example, may be a chip with various structures.
[0082] In the embodiment of the present application, the above application is to use the composition to perform surface treatment on semiconductors containing nitrogen-silicon bonds on the surface. For example, it can be used for grinding silicon nitride to increase the removal rate of silicon nitride. On the one hand, the modified particles in the embodiment of the present application composition can utilize their negative charge to generate a strong electrostatic attraction between the surface of the semiconductor substrate to be treated with positive charge, which is conducive to enhancing the mechanical grinding effect; at the same time, the negatively charged modified group can be used as a nucleophilic agent to attack the positively charged semiconductor substrate material, thereby facilitating the hydrolysis of the semiconductor substrate material and the breaking of the chemical bonds; the above two effects can greatly increase the removal rate of the semiconductor substrate material.
[0083] Accordingly, the embodiment of the present application also provides a semiconductor substrate, which is obtained by surface flattening the semiconductor substrate using the composition of the embodiment of the present application. In the embodiment of the present application, the semiconductor substrate can be a substrate to be flattened produced at each process node in the preparation of an electronic product, and the substrate obtained after surface flattening the composition of the embodiment of the present application. For example, the semiconductor substrate can be a chip with various structures. The shape, size, material composition, etc. of the semiconductor substrate are designed according to actual needs. The semiconductor substrate can include silicon nitride and / or silicon oxide, for example.
[0084] See also Figure 3 The present application also provides a semiconductor device 100, which includes the semiconductor substrate 111 described in the present application, and a functional layer 112 disposed on the semiconductor substrate 111. The functional layer 112 may be a film layer or component designed for various functional requirements of the semiconductor device 100, such as an electrode layer, a wiring layer, a conductor layer, etc. It should be noted that Figure 3It is only a schematic diagram of the cross-sectional structure of the semiconductor device 100 , and its specific structural design form is not limited.
[0085] The present application also provides a surface treatment method, which allows the above-mentioned composition to contact and grind the surface of the semiconductor substrate to be treated. The surface treatment method is a surface flattening treatment method, which uses the composition as a grinding liquid to grind the surface of the semiconductor substrate to be treated. By using the composition of the present application, the flattening treatment efficiency and the flattening treatment effect can be improved.
[0086] Taking the semiconductor substrate to be processed as a semiconductor substrate having silicon nitride on its surface as an example, specifically, the process of the surface treatment method of the embodiment of the present application includes: Figure 1 , the grinding pad 102 is flatly attached to the grinding table 101, the semiconductor substrate 103 to be processed is hung upside down on the grinding head 104, and the side surface containing silicon nitride to be ground is contacted with the grinding head 104, and then pressed on the grinding pad 102 rotating on the grinding table 101 with a certain pressure. The grinding head 104 starts to rotate with the semiconductor substrate 103, and the grinding table 101 also rotates at a certain speed. At the same time, the grinding liquid 105, i.e. the above-mentioned composition, is added to the grinding pad 102 at a certain rate and spreads flat with the centrifugal force. The semiconductor substrate 103 realizes the removal of silicon nitride under the dual action of chemistry and mechanics. After the above process is completed, the abrasive and organic matter remaining on the surface of the semiconductor substrate are removed by a post-cleaning process.
[0087] The embodiment of the present application also provides a modified particle dispersion for surface treatment of a semiconductor substrate, the modified particle dispersion comprising modified particles and a solvent, wherein the modified particles comprise oxide particles and a modified group represented by formula (1) bonded to the oxide particles;
[0088]
[0089] In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy;
[0090] The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
[0091] In the embodiments of the present application, the specific features of the modified particles are as described above and will not be repeated here. In the embodiments of the present application, the solvent may be water or the aforementioned organic solvent.
[0092] The modified particle dispersion of the embodiment of the present application can be used as an abrasive to prepare a planarization composition for surface planarization treatment of a semiconductor substrate. The modified particles in the modified particle dispersion are modified with negatively charged modified groups of a special structure, and can be used for grinding semiconductor substrates with positively charged surfaces, thereby increasing the removal rate of semiconductor substrate materials with positively charged surfaces, and can also enable the semiconductor substrate to obtain a lower defect value after surface planarization treatment.
[0093] The embodiments of the present application are further described below with reference to a plurality of embodiments.
[0094] Example 1
[0095] Add an appropriate amount of water to the modified colloidal silica, then add phosphoric acid as a pH regulator, and mix thoroughly under stirring to obtain a composition, in which the weight content of the modified particles is 0.5%, wherein the amount of phosphoric acid added is controlled so that the pH of the composition is stabilized to 2. The modified colloidal silica includes silica particles and a modified group shown in formula (1) bound to the silica particles; in formula (1), X is phosphorus; R1 is ethoxy, R2 is H, and R3 is -CH2-CH2-. The ratio of the number of phosphorus atoms to the number of silanol groups in the modified colloidal silica is 10%. The average particle size of the modified colloidal silica measured by dynamic light scattering is 70nm. The carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 10.5 atomic%.
[0096] Example 2
[0097] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is H, and R3 is -CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 6.1 atomic %.
[0098] Example 3
[0099] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is NH4, and R3 is -CH2-CH2-CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 8.9 atomic %.
[0100] Example 4
[0101] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is Na, and R3 is -CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 7.6 atomic %.
[0102] Example 5
[0103] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is K, and R3 is -CH2-CH2-CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 13.0 atomic %.
[0104] Example 6
[0105] The only difference from Example 1 is that in formula (1), X is phosphorus; R1 is methyl, R2 is methyl, and R3 is -CH2-CH2-CH2-; the carbon atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 11.2 atomic %.
[0106] Comparative Example 1.1
[0107] The only difference from Example 1 is that unmodified colloidal silica is used as the abrasive.
[0108] Comparative Example 2.1
[0109] The only difference from Example 1 is that commercial sulfonic acid group-modified colloidal silica is used as the abrasive.
[0110] The compositions of Examples 1 to 6, Comparative Example 1.1 and Comparative Example 2.1 were subjected to the following grinding test:
[0111] Grinding conditions: using a bench grinder, 1 psi pressure, 63 rpm platen speed, 57 rpm carrier speed, composition feed flow rate of 200 mL / min, using the composition to polish silicon nitride (SiN) substrate and silicon oxide (TEOS) substrate separately, and measuring the removal rate of the composition for different semiconductor substrates, RR is the removal rate. The film thickness of the semiconductor substrate before and after grinding is measured by a film thickness measuring device. The difference in film thickness before and after is divided by the grinding time to obtain the RR value. The selection ratio is the ratio of SiN RR to TEOS RR. The CANNA-600 wafer surface defect detection equipment of China Science and Technology Feice Company is used to measure the number of defects above 0.1μm on the grinding object, which is recorded as the defect value.
[0112] The grinding test results of the compositions of Examples 1 to 6, Comparative Examples 1.1 and 2.1 are shown in Table 1:
[0113] Table 1
[0114]
[0115] It can be seen from the results in Table 1 that, compared with the composition of Comparative Example 1 using unmodified silica as an abrasive and the composition of Comparative Example 2 using commercial sulfonic acid group-modified silica as an abrasive, the compositions of Examples 1 to 6 of the present application using colloidal silica modified with the modifying group shown in formula (1) as an abrasive exhibited a higher SiN removal rate, a higher SiN / TEOS selectivity, and also obtained lower SiN defect and TEOS defect values.
[0116] Example 7
[0117] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 0.5%, and the P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 0.21 atomic %.
[0118] Example 8
[0119] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 4.7%, and the P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 2.4 atomic %.
[0120] Example 9
[0121] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 22%, and the P atoms in the modified colloidal silica measured by X-ray photoelectron spectroscopy are 8.1 atomic %.
[0122] Example 10
[0123] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 46%, and the P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 23.5 atomic %.
[0124] Embodiment 11
[0125] The only difference from Example 2 is that the ratio of phosphorus atoms to silanol groups in the modified colloidal silica is 0.3%, and the P atom content of the modified colloidal silica measured by X-ray photoelectron spectroscopy is 0.13 atomic %.
[0126] The compositions of Examples 7 to 11 were subjected to grinding tests, and the test results are shown in Table 2:
[0127] Table 2
[0128]
[0129] According to the results in Table 2, by comparing Example 2 and Examples 7-11, it can be seen that when the content of the modified groups on the surface of colloidal silica in the planarization composition is kept within a certain range, it is beneficial to promote the improvement of SiN RR or SiN / TEOS selectivity. When the amount of modified groups on the surface of silica in the planarization composition exceeds the appropriate ratio, it is not beneficial to further increase SiN RR or SiN / TEOS selectivity.
[0130] Example 12
[0131] The only difference from Example 2 is that the pH of the composition was adjusted to 3.
[0132] Embodiment 13
[0133] The only difference from Example 2 is that the pH of the composition is adjusted to 4.
[0134] Embodiment 14
[0135] The only difference from Example 2 is that the pH of the composition is adjusted to 5.
[0136] Embodiment 15
[0137] The only difference from Example 2 is that the pH of the composition was adjusted to 6.
[0138] Comparative Example 1.2
[0139] The only difference from Example 12 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0140] Comparative Example 1.3
[0141] The only difference from Example 13 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0142] Comparative Example 1.4
[0143] The only difference from Example 14 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0144] Comparative Example 1.5
[0145] The only difference from Example 15 is that unmodified colloidal silica is used as the abrasive with an average particle size of 70 nm.
[0146] Comparative Example 2.2
[0147] The only difference from Example 12 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0148] Comparative Example 2.3
[0149] The only difference from Example 13 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0150] Comparative Example 2.4
[0151] The only difference from Example 14 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0152] Comparative Example 2.5
[0153] The only difference from Example 15 is that commercial sulfonic acid-modified colloidal silica is used as the abrasive, and the average particle size is 70 nm.
[0154] The compositions of Examples 12 to 15, Comparative Examples 1.1 to 1.5, and Comparative Examples 2.1 to 2.5 were subjected to grinding tests, and the test results are shown in Table 3. The potential of the composition was measured using a Zeta potential meter according to the electrophoretic light scattering method.
[0155] Table 3
[0156]
[0157] It can be seen from the results of Table 3 that in the range of pH 2-6, compared with the planarization compositions of Comparative Examples 1.1 to 1.5, and Comparative Examples 2.1 to 2.5, the planarization compositions prepared by modified particles modified with specific modifying groups provided in Example 2 of the present application, and Examples 12 to 15, all exhibited higher SiN removal rates and higher SiN / TEOS selectivities under different pH conditions. Among them, it can be seen from Comparative Example 2, and Examples 12 to 15 that when the pH is 2, the composition has a higher SiN RR, and as the pH increases, the SiN RR decreases, indicating that the pH value of the composition has a greater effect on the SiN removal rate. In addition, it can be seen from Example 2, and Examples 12 to 15 that compared with the composition of Example 15 with a pH of 6, the compositions of Example 2, and Examples 12 to 14 have a higher SiN / TEOS selectivity.
[0158] Compared with the planarization compositions using unmodified colloidal silica of Comparative Examples 1.1 to 1.5, the planarization compositions of Example 2 and Example 12 to Example 15 of the present application exhibit a higher SiN removal rate and a higher SiN / TEOS selectivity ratio. This is because the colloidal SiO2 surface in the planarization compositions of the present application embodiments is modified with negatively charged specific modifying groups, which can effectively improve the SiN RR.
[0159] Compared with the planarization compositions of Comparative Examples 2.1 to 2.5 using commercial sulfonic acid group-modified colloidal silica, the planarization compositions of Example 2, and Example 12 to Example 15 of the present application exhibit a higher SiN removal rate and a higher SiN / TEOS selectivity ratio, which strongly proves that the planarization composition of colloidal silica modified with specific groups provided in the present application is extremely competitive in promoting SiN RR and is more conducive to promoting the polishing removal of SiN.
[0160] Example 16
[0161] The only difference from Example 2 is that citric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0162] Embodiment 17
[0163] The only difference from Example 2 is that nitric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0164] Comparative Example 1.6
[0165] The only difference from Comparative Example 1.1 is that citric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0166] Comparative Example 1.7
[0167] The only difference from Comparative Example 1.1 is that nitric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0168] Comparative Example 2.6
[0169] The only difference from Comparative Example 2.1 is that citric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0170] Comparative Example 2.7
[0171] The only difference from Comparative Example 2.1 is that nitric acid is used as a pH adjuster to adjust the pH of the composition to 2.
[0172] The compositions of Examples 16 and 17 and Comparative Examples 2.6 and 2.7 were subjected to the aforementioned grinding test. The test results are listed in Table 4.
[0173] Table 4
[0174]
[0175]
[0176] It can be seen from the results in Table 4 that when different organic acids or inorganic acids are used as pH adjusters, the planarization compositions prepared by using modified particles modified with specific modifying groups provided in Examples 2, 16 and 17 of the present application, compared with the planarization compositions containing unmodified silicon dioxide in Comparative Examples 1.1, 1.6 and 1.7, and the planarization compositions of commercial sulfonic acid-modified silicon dioxide in Comparative Examples 2.1, 2.6 and 2.7, show higher SiN removal rates and higher SiN / Ox selectivities, indicating that the planarization compositions prepared by using modified particles modified with specific modifying groups provided in the present application, when different types of inorganic acids and organic acids are used as pH adjusters, are beneficial to significantly promote the improvement of SiN RR.
[0177] Embodiment 18
[0178] The only difference from Example 12 is that the weight content of the modified particles in the composition is 4%.
[0179] Comparative Example 2.8
[0180] The only difference from Example 2 is that the weight content of the commercial sulfonic acid-modified silica particles in the composition is 4%.
[0181] The parameter characteristics and grinding test results of the compositions of Example 2, Example 12, Example 18, Comparative Example 2.1, Comparative Example 2.2, and Comparative Example 2.8 are listed in Table 5.
[0182] Table 5
[0183]
[0184] As can be seen from the results of Table 5, when the content of abrasive in the composition increases, the SiN RR can be significantly increased by comparing Example 12 with Example 18. Compared with the planarization compositions containing commercial sulfonic acid group-modified silica in Comparative Examples 2.1, 2.2 and 2.8, the planarization compositions provided in the present application exhibit higher SiN removal rates and higher SiN / Ox selectivity ratios under low and high concentration abrasive content conditions, which fully demonstrates that the planarization compositions containing silica modified with specific structural modifying groups provided in the present application can effectively remove SiN under a wide range of abrasive concentration conditions.
[0185] In addition, it can be seen from the results in Table 5 that the planarization composition of the present application exhibits lower SiN defect and Ox defect values than the planarization composition containing commercial sulfonic acid modified silica, which is specifically manifested in that there are fewer surface particles remaining in the grinding layer after grinding and it is easier to clean. This is mainly due to the low degree of ionization of the modified groups on the modified silica in the embodiments of the present application, so that the planarization composition of the embodiments of the present application exhibits lower surface residue and easier cleaning characteristics.
[0186] The planarization compositions of Examples 1-18 of the present application have relatively low viscosity and relatively high water content, the viscosity of the compositions at 25° C. is in the range of 1 centipoise to 10 centipoise, and the water content is in the range of 80% to 99.3%. The viscosity of the compositions can be measured using a viscometer.
[0187] It should be understood that the first, second and various numerical numbers involved in this document are only distinguished for the convenience of description and are not used to limit the scope of the present application.
[0188] In this application, "and / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone, where A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0189] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0190] In the present application, “-” represents a range value, including the endpoint values at both ends. For example, the average particle size of the modified particles is 5nm-500nm, which means that the average particle size of the modified particles is between 5nm and 500nm, and includes the endpoint values 5nm and 500nm.
[0191] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
Claims
1. A composition, characterized in that The composition comprises modified particles, a pH adjuster and a solvent, wherein the modified particles comprise oxide particles and a modifying group represented by formula (1) bonded to the oxide particles; In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy; The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
2. The composition according to claim 1, characterized in that The content of X atoms in the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 0.01 atomic % and less than or equal to 30 atomic %.
3. The composition according to claim 1 or 2, characterized in that The carbon atom content of the modified particles measured by X-ray photoelectron spectroscopy is greater than or equal to 2 atomic % and less than or equal to 45 atomic %.
4. The composition according to any one of claims 1 to 3, characterized in that The oxide particles are silicon dioxide particles, and the ratio of the number of X atoms to the number of silanol groups in the modified particles is greater than or equal to 0.4% and less than or equal to 48%.
5. The composition according to any one of claims 1 to 4, characterized in that The modifying group is bonded to the oxide particle by chemical bonding.
6. The composition according to any one of claims 1 to 5, characterized in that The average particle size of the modified particles measured by dynamic light scattering method is 5nm-500nm.
7. The composition according to any one of claims 1 to 6, characterized in that In the composition, the weight proportion of the modified particles is 0.1%-50%.
8. The composition according to any one of claims 1 to 7, characterized in that The pH of the composition is less than 12.
9. The composition according to claim 8, characterized in that The pH of the composition is 1-6.
10. The composition according to any one of claims 1 to 9, characterized in that The average association degree of the modified particles is 1-10.
11. The composition according to any one of claims 1 to 10, characterized in that The potential of the composition is in the range of -55 to -5.
12. The composition according to any one of claims 1 to 11, characterized in that The substituted or unsubstituted alkyl group is a substituted or unsubstituted C1-C6 alkyl group, the substituted or unsubstituted alkoxy group is a substituted or unsubstituted C1-C6 alkoxy group; the substituted or unsubstituted alkylene group is a substituted or unsubstituted C1-C6 alkylene group, and the substituted or unsubstituted alkyleneoxy group is a substituted or unsubstituted C1-C6 alkyleneoxy group.
13. The composition according to any one of claims 1 to 12, characterized in that The pH adjuster includes an acid, or a combination of an acid and a base or a base salt, and the acid includes an organic acid and / or an inorganic acid.
14. The composition according to any one of claims 1 to 13, characterized in that The solvent includes water or an organic solvent.
15. The composition according to any one of claims 1 to 14, characterized in that The composition further comprises one or more of a catalyst, an oxidant, a surfactant, a preservative, a passivator, and a reducing agent.
16. The composition according to any one of claims 1 to 15, characterized in that The mass content of the solvent in the composition is greater than or equal to 50% and less than 100%.
17. The composition according to any one of claims 1 to 16, characterized in that The viscosity of the composition at 25° C. is 1 centipoise to 80 centipoise.
18. The composition according to any one of claims 1 to 17, characterized in that The removal rate of silicon nitride by the composition is greater than 19. The composition according to any one of claims 1 to 18, characterized in that The removal selectivity of the composition to silicon nitride and silicon oxide is greater than 1.
5.
20. Use of the composition according to any one of claims 1 to 19 in surface treatment of a semiconductor substrate.
21. The use according to claim 20, characterized in that The composition is used to treat the surface of a semiconductor substrate with positive surface charge.
22. The use according to claim 21, characterized in that The composition is used to perform surface treatment on a semiconductor substrate containing nitrogen-silicon bonds on the surface.
23. A surface treatment method, characterized in that: The composition according to any one of claims 1 to 19 is brought into contact with and polished on the surface of a semiconductor substrate to be processed.
24. A modified particle dispersion for surface treatment of a semiconductor substrate, characterized in that: The modified particle dispersion comprises modified particles and a solvent, wherein the modified particles comprise oxide particles and a modified group represented by formula (1) bonded to the oxide particles; In formula (1), X is selected from phosphorus, arsenic, antimony, and bismuth; R1 is selected from substituted or unsubstituted alkyl, substituted or unsubstituted alkoxy, substituted or unsubstituted aryl, and substituted or unsubstituted aryloxy; R2 is selected from H, NH4, Li, Na, K, substituted or unsubstituted alkyl, and substituted or unsubstituted aryl; R3 is selected from substituted or unsubstituted alkylene, substituted or unsubstituted alkyleneoxy, substituted or unsubstituted arylene, and substituted or unsubstituted aryleneoxy; The oxide particles include any one of silicon dioxide particles, aluminum oxide particles, zinc oxide particles, titanium dioxide particles, zirconium dioxide particles, and cerium oxide particles.
25. A semiconductor substrate, characterized in that: The semiconductor substrate is obtained by subjecting the surface of the semiconductor substrate to a planarization treatment using the composition described in any one of claims 1 to 19.
26. The semiconductor substrate according to claim 25, wherein: The semiconductor substrate includes silicon nitride and / or oxide.