Anisotropic conductive adhesive film as well as preparation method and application thereof
By reacting acrylate phosphate monomer with epoxy resin to form a new resin, combined with filler particles and initiator, the problems of poor conduction and curing shrinkage in the heterosquamous conductive adhesive film are solved, and the bonding strength is improved and High temperature and high humidity performance ensures the stability and performance of the product.
Patent Information
- Application Number
- CN202410950724.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-12-03
AI Technical Summary
During use, existing heterosqualitative conductive adhesive films have poor conduction, bubble problems caused by curing and shrinking, unclear indentation, insufficient interface bonding strength, and post-reliability problems.
Using raw materials such as rubber, acrylic resin, epoxy resin, polyurethane, acrylate phosphate monomer and conductive particles, a new thermosetting resin is formed by reacting acrylate phosphate monomer with epoxy resin, combining filler particles and initiator to prepare A heterosquamous conductive adhesive film without curing agent is produced, and the bonding strength and conduction performance are improved through specific coating and curing treatment methods.
It effectively reduces the generation of bubbles during curing, improves conduction performance and bonding strength, enhances adhesion and high temperature and high humidity performance, and ensures the stability and reliability of the product to maintain excellent performance.
Smart Images

Figure BDA0004947159740000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of conductive adhesive films and relates to an anisotropic conductive adhesive film and a preparation method and application thereof. Background Art
[0002] With the rapid progress of modern society, the scientific and technological revolution has profoundly changed people's lifestyles and working patterns. Electronic products, such as smart phones, tablets, laptops and even various smart wearable devices, have become an indispensable part of modern life. As an important component of electronic products, liquid crystal display screens, anisotropic conductive film (ACF) is an important material to ensure its display effect and product reliability. ACF is a special material that integrates insulation, conductivity and bonding functions. Its unique performance lies in the ability to achieve precise conductive connections in the vertical direction while maintaining insulation in the horizontal direction. This feature is crucial to ensure the safe operation of the internal circuits of the display screen. The application of ACF makes signal transmission stable and efficient while avoiding the risk of short circuits.
[0003] ACF is mainly composed of conductive particles and adhesives. Conductive particles are usually made of metal or metal-coated polymer materials. Under the action of pressure and heating, they can be precisely arranged in the vertical direction to form microscopic conductive bridges, ensuring that the current can flow stably and efficiently between the two connected electronic components. As another core component of ACF, the adhesive plays a vital role; it not only firmly fixes the conductive particles between the two connecting surfaces to form a stable electrical connection, but also provides sufficient mechanical strength to ensure that the ACF can still maintain good adhesion and stability in complex use environments. The adhesive is mainly composed of thermoplastic elastomers, thermosetting resins and curing agents. Thermoplastic elastomers generally do not participate in the reaction, melt at low temperature, and initially have a bonding effect. Thermosetting resins commonly used are epoxy resins and free radical polymerization resins, among which epoxy resins are the most commonly used, mainly bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, phenoxy resin, etc. Free radical polymerization resins mainly include acrylates, polyurethane acrylates, epoxy acrylates, amine-modified bismaleimide resins, unsaturated polyamide resins, etc., which are initiated by initiators. Curing agents commonly use latent imidazole curing agents. Under heating or other specific conditions, imidazole curing agents will be activated, catalyzing the ring-opening polymerization of epoxy groups in epoxy resins to form a cross-linked structure, thereby completing curing.
[0004] The ACF currently prepared will have the following problems more or less due to different usage scenarios: 1. Poor conduction; 2. Bubble problems caused by ACF curing shrinkage; 3. Unclear indentation; 4. Insufficient bonding strength between interfaces; 5. After reliability, the indentation disappears and product performance problems occur. ACF researchers are constantly working to improve the formula and production technology of ACF in order to overcome the above problems. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the object of the present invention is to provide an anisotropic conductive adhesive film and a preparation method and application thereof.
[0006] One object of the present invention is achieved by the following technical solutions:
[0007] The invention discloses an anisotropic conductive adhesive film, wherein the raw materials include, by weight percentage, 20-40% rubber, 5-20% acrylic resin, 5-20% epoxy resin, 5-20% polyurethane, 2-15% monomer, 1-5% initiator and 2-7% conductive particles.
[0008] Preferably, the monomer is an acrylate phosphate; an acrylate phosphate is a compound containing a phosphate group and an acrylate group.
[0009] More preferably, the acrylate phosphate is polyethylene glycol monomethacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, 2-hydroxyethyl methacrylate phosphate, SIPOMER PAM200, KM2110, or KM2130.
[0010] More preferably, the acrylate phosphate is di(methacryloyloxyethyl) hydrogen phosphate, such as KM2120 produced by Hangzhou Furuide.
[0011] Preferably, the rubber is one or more of styrene-butadiene rubber or its modified substance, nitrile-butadiene rubber or its modified substance, chloroprene rubber or its modified substance, butadiene rubber or its modified substance, isoprene rubber or its modified substance.
[0012] Preferably, the epoxy resin includes one or more of glycidyl ether epoxy resin (such as bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, phenolic resin, etc.), glycidyl amine epoxy resin, and glycidyl ester epoxy resin.
[0013] Preferably, the initiator is a thermal initiator, and the thermal initiator includes one or more of a peroxide initiator, an azo initiator, and a redox initiator system.
[0014] Peroxide initiators may be one or more of dibenzoyl peroxide, diisopropylbenzene hydroperoxide, diisopropylbenzene peroxide, tert-butyl hydroperoxide, and di-tert-butyl peroxide. Azo initiators may be azobisisobutyronitrile and azobisisoheptylnitrile. Redox initiator systems are systems composed of oxidants and reductants, oxidants may be persulfates, peroxides, dichromates, etc., and reductants may be sulfites, iron salts, ascorbic acid, etc.
[0015] Preferably, the conductive particles are a core-shell structure composition with a polymer as the core and a metal layer as the shell, the polymer can be listed as one or more of polymethyl methacrylate, polyaniline, polystyrene, polyacrylamide, polyvinyl chloride, and polyacrylonitrile, and the metal layer can be listed as one or more of nickel layer, gold layer, copper layer, and cobalt layer.
[0016] More preferably, the particle size of the conductive particles is 0.5 to 20 μm, and further preferably 1 to 8 μm.
[0017] Preferably, the raw material further comprises 8-30% filler particles by weight.
[0018] Preferably, the filling particles are one or more of silicon dioxide, titanium dioxide, aluminum oxide, zirconium oxide, and magnesium oxide.
[0019] Preferably, the raw materials also include other additives, and other additives are not particularly limited, and any additive that can be used in the anisotropic conductive adhesive film to modify the function can be used, and can be listed as colorants, adhesion promoters, antioxidants, and the like.
[0020] The anisotropic conductive adhesive film of the present invention does not include a curing agent.
[0021] The second object of the present invention is achieved by the following technical solutions:
[0022] The method for preparing the anisotropic conductive adhesive film comprises the following steps:
[0023] The monomer, epoxy resin, polyurethane, acrylic resin and rubber are added to the solvent and mixed evenly, and then the filling particles are added and mixed, and finally the conductive particles and initiator are added and stirred to prepare the coating liquid, and the anisotropic conductive adhesive film is obtained after coating and drying.
[0024] Preferably, the solvent can be listed as benzene solvents (toluene, benzene, etc.), ketone solvents (methyl ethyl ketone, acetone, butanone, etc.), alcohol solvents (ethanol, isopropanol, etc.), ester solvents (ethyl acetate, butyl acetate, etc.), etc.
[0025] Preferably, the solid content of the coating liquid is 30-60 wt %.
[0026] The third object of the present invention is achieved by the following technical solutions:
[0027] The application of the anisotropic conductive adhesive film comprises: placing the anisotropic conductive adhesive film between two electronic components, and then bonding the two electronic components through a curing process.
[0028] Preferably, the curing temperature is 130-180° C., and the minimum curing temperature is 130° C.; the curing pressure is 0.5-10 MPa, and more preferably 1-5 MPa; and the curing time is 2-10 s, and more preferably 3-6 s.
[0029] Preferably, after the curing treatment at a curing temperature of 150° C., a curing pressure of 3 MPa, and a curing time of 4 s, the curing rate of the anisotropic conductive adhesive film is ≥85%, the bonding strength is ≥1500 gf / cm, and the on-resistance is ≤0.95Ω.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The raw materials of the anisotropic conductive film of the present invention include: rubber, acrylic resin, epoxy resin, polyurethane, acrylate phosphate monomer, initiator, conductive particles, and filler particles. By using acrylate phosphate monomer, the acrylate phosphate monomer can react with the epoxy resin in the system to form a new thermosetting resin without the traditional epoxy curing agent, thereby improving the overall performance of the ACF.
[0032] 2. The ingenious anisotropic conductive adhesive film system of the present invention adopts acrylate phosphate monomers, which can stably coexist with epoxy resin under low temperature conditions, and react with epoxy resin under heating conditions to obtain a new epoxy ring-opened resin containing acrylic acid and phosphoric acid. The new epoxy ring-opened resin containing acrylic acid and phosphoric acid can continue to react with the acrylic resin and polyurethane in the system under the initiation of an initiator, and cross-link and cure, which can effectively reduce the shrinkage of acrylate and polyurethane during the cross-linking and curing process, and reduce the generation of bubbles during the curing process, so that the poor appearance of the product is reduced, the indentation is clear, and the conductive performance is improved.
[0033] 3. The present invention adopts acrylate phosphate monomers, which react with the various ingredients in the formula during the heating process to obtain a new anisotropic conductive adhesive film. The ACF has a lower operating temperature than the ACF obtained by the pure epoxy system; the anisotropic conductive adhesive film has good adhesion, and the bonding strength between the electrode is enhanced; the anisotropic conductive adhesive film has excellent high temperature and high humidity resistance, and the stability and reliability are improved, which greatly reduces the poor conduction caused by the increase of the Gap value after the reliability.
[0034] 4. The anisotropic conductive adhesive film of the present invention maintains excellent performance after reliability testing and has wide applicability. DETAILED DESCRIPTION
[0035] The technical scheme of the present invention is further described below by specific embodiments. It should be understood that the specific embodiments described herein are only used to help understand the present invention and are not intended to be used for specific limitations of the present invention. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.
[0036] Conductive particles: nickel-plated polystyrene microspheres, average particle size 5 μm, Zhenjiang Aibang Ni-500;
[0037] Carboxyl-modified butadiene rubber was purchased from Sinopec, and the degree of carboxyl substitution was approximately 25%;
[0038] Acrylic resin and polyurethane were purchased from Miwon Trading Co., Ltd. of South Korea.
[0039] Example 1
[0040] The raw materials of the anisotropic conductive film of this embodiment are: 23 parts of carboxyl-modified butadiene rubber; 10 parts of acrylic resin; 16 parts of polyurethane; 12 parts of bisphenol A epoxy resin (E54); 24 parts of filler particles (alumina); 4 parts of monomer (KM2120); initiator (4 parts of dibenzoyl peroxide, 1 part of diisopropylbenzene hydroperoxide); and 6 parts of conductive particles.
[0041] The preparation method of anisotropic conductive adhesive film includes: at room temperature, firstly, monomer, E54 bisphenol A epoxy resin, polyurethane, acrylic resin, and carboxyl modified butadiene rubber are sequentially added to a mixer containing toluene and stirred evenly; filling particles are added for dispersion and stirred evenly; finally, conductive particles and initiator are added and stirred evenly to obtain a coating liquid (solid content is 50wt%), the coating liquid is filtered with a filter element, and then coated on a coating machine, the oven temperature during the coating process is 70°C, and the ACF is dried to obtain a final anisotropic conductive adhesive film with a thickness of 20μm.
[0042] Example 2
[0043] The raw materials of the anisotropic conductive film of this embodiment are: 28 parts of carboxyl-modified butadiene rubber; 8 parts of acrylic resin; 13 parts of polyurethane; 15 parts of bisphenol F epoxy resin (370); 21 parts of filler particles (titanium dioxide); 6 parts of monomer (SIPOMER PAM100); 4 parts of initiator (diisopropylbenzene hydroperoxide); and 5 parts of conductive particles.
[0044] The preparation method of anisotropic conductive adhesive film includes: firstly, monomer, 370 bisphenol F type epoxy resin, polyurethane, acrylic resin, and carboxyl modified butadiene rubber are added to a mixer containing toluene in sequence and stirred evenly; filler particles are added for dispersion and stirred evenly; finally, conductive particles and initiator are added and stirred evenly to obtain a coating liquid (solid content is 45wt%), the coating liquid is filtered with a filter element, and then coated on a coating machine, the oven temperature during the coating process is 70°C, and the ACF is dried to obtain a final anisotropic conductive adhesive film with a thickness of 20μm.
[0045] Example 3
[0046] The raw materials of the anisotropic conductive film of this embodiment are: 25 parts of carboxyl-modified butadiene rubber; 13 parts of acrylic resin; 10 parts of polyurethane; 16 parts of bisphenol A epoxy resin (E51); 17 parts of filler particles (zirconium oxide); 8 parts of monomer (SIPOMER PAM200); 4 parts of initiator (azobisisobutyronitrile); and 7 parts of conductive particles.
[0047] The preparation method of anisotropic conductive adhesive film includes: firstly, monomer, E51 bisphenol A epoxy resin, polyurethane, acrylic resin, and carboxyl modified butadiene rubber are added to a mixer containing toluene in sequence and stirred evenly; filler particles are added for dispersion and stirred evenly; finally, conductive particles and initiator are added and stirred evenly to obtain a coating liquid (solid content is 55wt%), the coating liquid is filtered with a filter element, and then coated on a coating machine, the oven temperature during the coating process is 70°C, and the ACF is dried to obtain a final anisotropic conductive adhesive film with a thickness of 20μm.
[0048] Comparative Example 1
[0049] The difference between Comparative Example 1 and Example 1 is that no monomer is added in Comparative Example 1. In Comparative Example 1, E54 bisphenol A epoxy resin, polyurethane, acrylic resin, and carboxyl-modified butadiene rubber are added to a mixer containing toluene in sequence and stirred evenly. The rest is the same as Example 1.
[0050] Comparative Example 2
[0051] The difference between Comparative Example 2 and Example 1 is that, instead of using KM2120, pentaerythritol triacrylate is used as a monomer in Comparative Example 2, and the rest is the same as Example 1.
[0052] Comparative Example 3
[0053] The difference between Comparative Example 3 and Example 1 is that, in Comparative Example 3, E54 bisphenol A epoxy resin is not added. In Comparative Example 3, monomer, polyurethane, acrylic resin, and carboxyl-modified butadiene rubber are added to a mixer containing toluene in sequence and stirred evenly. The rest is the same as Example 1.
[0054] Comparative Example 4
[0055] The difference between Comparative Example 4 and Example 1 is that, instead of using monomers, 10 parts of capsule-type 2-ethylimidazole curing agent (Hubei Yamade) were added in Comparative Example 4, and the rest was the same as Example 1.
[0056] Comparative Example 5
[0057] The difference between Comparative Example 5 and Example 1 is that 10 parts of capsule-type 2-ethylimidazole curing agent (Hubei Yamade) are further added to Comparative Example 5, and the rest is the same as Example 1.
[0058] The anisotropic conductive adhesive films of Examples 1-3 and Comparative Examples 1-5 were cured using a Bonder device under the curing conditions of 3MPa and 4s. Binding was performed at different temperatures to determine the lowest curing temperature. After binding at 3MPa, 4s, and 150°C (Comparative Example 4 was bound at 160°C, and other embodiments and comparative example groups were bound at 150°C), a peel strength tester was used to measure the bonding force (gf / cm) at a peeling angle of 90° and a peeling speed of 50mm / min; a pre-designed electrode with detectable on-resistance was selected on the FPC, and an on-resistance test was performed using a resistance meter. After binding, the electrodes were aged for 500 hours at 85°C and 85% humidity, and then the on-resistance and bonding force after trust were determined. The test results are shown in Table 1.
[0059] Table 1 Performance test results of anisotropic conductive adhesive films of Examples 1-3 and Comparative Examples 1-4
[0060]
[0061] *The higher the bubble score, the smaller the number of bubbles and the smaller the bubble volume;
[0062] *The higher the indentation score, the more uniform and stronger the indentation mark.
[0063] It can be seen from Table 1 that the anisotropic conductive adhesive films obtained in Examples 1-3 can effectively reduce the generation of bubbles during the curing process, reduce the poor appearance of the product, and make the indentation clearer; the anisotropic conductive adhesive films of Examples 1-3 have a lower curing temperature, good adhesion and excellent high temperature and high humidity resistance, and the stability and reliability are improved.
[0064] In Comparative Example 1, no acrylate phosphate monomer was added, which affected the product appearance, bonding strength, on-resistance and reliability stability; in Comparative Example 2, conventional pentaerythritol triacrylate was added as a monomer, and under heating conditions, pentaerythritol triacrylate polymerized with the epoxy resin under the initiation of the initiator, and did not form the "new epoxy ring-opened resin containing acrylic acid and phosphoric acid" of the present invention. Therefore, the product appearance, bonding strength and on-resistance of Comparative Example 2 were affected; in Comparative Example 3, no epoxy resin was added, and the product performance was reduced; in Comparative Example 4, no monomer was added, but a conventional curing agent was added, and the curing temperature of the system was greatly increased; in Comparative Example 5, a curing agent was added after the monomer was added, and the curing rate was too fast, and the attached bubbles were not discharged, affecting the appearance and reliability stability.
[0065] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0066] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.
[0067] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.
Claims
1. An anisotropic conductive film, characterized in that: The raw materials include, by weight percentage, 20-40% rubber, 5-20% acrylic resin, 5-20% epoxy resin, 5-20% polyurethane, 2-15% monomer, 1-5% initiator, and 2-7% conductive particles.
2. The anisotropic conductive adhesive film according to claim 1, characterized in that: The monomers are acrylate phosphate esters.
3. The anisotropic conductive adhesive film according to claim 2, characterized in that: The acrylate phosphate is polyethylene glycol monomethacrylate phosphate, di(methacryloyloxyethyl) hydrogen phosphate, 2-hydroxyethyl methacrylate phosphate, SIPOMER PAM 200, KM2110, KM2130.
4. The anisotropic conductive adhesive film according to claim 1, characterized in that: The rubber is one or more of styrene-butadiene rubber or its modified substance, nitrile-butadiene rubber or its modified substance, chloroprene rubber or its modified substance, butadiene rubber or its modified substance, isoprene rubber or its modified substance; And / or, the epoxy resin includes one or more of glycidyl ether epoxy resin, glycidyl amine epoxy resin, and glycidyl ester epoxy resin; And / or, the initiator is a thermal initiator, and the thermal initiator includes one or more of a peroxide initiator, an azo initiator, and a redox initiator system.
5. The anisotropic conductive adhesive film according to claim 1, characterized in that: The raw material also includes 8-30% filler particles by weight.
6. The anisotropic conductive adhesive film according to claim 5, characterized in that: The filling particles are one or more of silicon dioxide, titanium dioxide, aluminum oxide, zirconium oxide, and magnesium oxide.
7. The method for preparing anisotropic conductive adhesive film according to claim 1, characterized in that: The preparation method comprises the following steps: The monomer, epoxy resin, polyurethane, acrylic resin and rubber are added to the solvent and mixed evenly, and then the filling particles are added and mixed, and finally the conductive particles and initiator are added and stirred to prepare the coating liquid, and the anisotropic conductive adhesive film is obtained after coating and drying.
8. The use of anisotropic conductive adhesive film according to claim 1, characterized in that: The application includes: arranging the anisotropic conductive adhesive film between two electronic components, and then achieving the bonding of the two electronic components through a curing process.
9. The use according to claim 8, characterized in that: The minimum curing temperature is 130-180°C, the curing pressure is 0.5-10MPa, and the curing time is 2-10s.
10. The use according to claim 8, characterized in that: After the curing treatment at a curing temperature of 150° C., a curing pressure of 3 MPa, and a curing time of 4 seconds, the curing rate of the anisotropic conductive adhesive film is ≥85%, the bonding strength is ≥1500 gf / cm, and the on-resistance is ≤0.95Ω.