Preparation method of coating protection glue with moisture-proof function

By detecting the performance of coated protective glue and adjusting the raw material ratio, the product quality instability caused by inconsistent raw material quality in the production of coated protective glue is solved, and the product performance improvement and raw material consumption optimization are achieved.

CN119060655AInactive Publication Date: 2024-12-03SHENZHEN AIBANG NEW MATERIAL TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411176318.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

During the production process of existing coated protective glue, product quality is inconsistent due to the differences in raw material quality between different origins or raw material manufacturers, and the lack of timely preparation method adjustments, resulting in uneven product quality.

Method used

A liquid rubber material is dissolved in xylene, and after heating, lubricant and α-hydroxybenzotriazole are added, loess is roasted and ground into powder, and after mixing, tackifier, initiator and zinc oxide are added, stirred to form coating. Cover the protective glue, and by testing its drying, strength, viscosity and waterproof properties, adjust the raw material ratio according to the test results to improve product quality.

Benefits of technology

By detecting and adjusting the raw material ratio, ensure the product performance is qualified, avoid defective products outflow, reduce raw material consumption, and improve production consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060655A_ABST
    Figure CN119060655A_ABST
Patent Text Reader

Abstract

The invention relates to the field of material science, in particular to a preparation method of coating protection glue with a moisture-proof function, which comprises the following steps: dissolving a liquid rubber material in xylene at normal temperature, and heating to 70-80 DEG C; adding a lubricant into the solution, stirring for 1-2 hours, adding alpha-hydroxybenzotriazole, and stirring for 1-2 hours; the preparation method comprises the following steps: roasting loess at 600-700 DEG C, cooling, and grinding into powder; heating the tackifier to 50-60 DEG C, adding the initiator, the waterproof agent and the zinc oxide, stirring for 30-40 minutes, adding the alpha-cyanoacrylate, and continuously stirring for 1-2 hours; mixing and stirring the products to obtain coating protective glue; and various properties of the coated protective glue are detected. According to the invention, various performances of the protective glue are evaluated by setting various performance indexes, and various data of the protective glue are obtained through various tests, so that whether various performances of the produced protective glue are qualified or not can be judged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of materials science, and in particular to a method for preparing a coating protective glue with moisture-proof function. Background Art

[0002] The coating protective glue industry is also called "TUFFY glue". TUFFY glue is a rubber system product that is mainly waterproof, salt spray, acid and alkali resistant. The product contains solvents. Rubber is dissolved in the solvent and a certain amount of resin is added to act as a bond. After the solvent in the product evaporates, the remaining effective ingredients will self-adhere and finally form a thin film, thereby playing the role of waterproofing, salt spray, acid and alkali resistant.

[0003] For example, the prior art disclosed in CN86101754A discloses a method for preparing a waterproof coating adhesive, which comprises adding crushed edges and waste plastics into coal tar preheated to 49-60°C in a boiling kettle, stirring and mixing, and heating to 110-150°C to melt the mixture. While heating, fillers, stabilizers and plasticizers are added in sequence.

[0004] Another typical prior art disclosed in CN109679574B is an acidic silicone coating adhesive and a preparation method thereof, wherein the components of the silicone rubber sealant are specifically composed of 100 parts by weight of α,ω-dihydroxypolydimethylsiloxane, 0 to 30 parts of dimethyl silicone oil, 2 to 20 parts of fumed silica, 3 to 10 parts of a cross-linking agent, and 0.1 to 3 parts of a catalyst.

[0005] Let's look at a rubber asphalt waterproof coating and a preparation method thereof disclosed in the prior art such as CN112063303A. Based on the total weight of the rubber asphalt waterproof coating, the rubber asphalt waterproof coating includes: 13-69wt% asphalt, 1-20wt% processing oil, 7-18wt% rubber modifier, 10-50wt% filler, 0.1-2.0wt% stabilizer and 0.1-5.0wt% coating agent.

[0006] At present, in the preparation method of the coating protective glue, the performance of the coating protective glue produced by raw materials purchased from different origins or raw material suppliers will be different. In the prior art, the preparation method is generally not adjusted in time according to the product quality, resulting in uneven quality of the products produced. In order to solve the common problems in the field, the present invention is made. Summary of the invention

[0007] The purpose of the present invention is to address the existing deficiencies and provide a method for preparing a coating protective adhesive with moisture-proof function.

[0008] In order to overcome the shortcomings of the prior art, the present invention adopts the following technical solutions:

[0009] A method for preparing a coating protective adhesive with moisture-proof function comprises the following steps:

[0010] S1, dissolving the liquid rubber material in xylene at room temperature and heating it to 70-80 degrees Celsius;

[0011] S2, add lubricant to the solution of S1 and stir for one to two hours, add α-hydroxybenzotriazole and stir for one to two hours;

[0012] S3, calcining the loess at 600-700 degrees Celsius, and grinding it into powder after cooling;

[0013] S4, heating the tackifier to 50-60 degrees Celsius, adding the initiator, waterproofing agent and zinc oxide, stirring for 30-40 minutes, and then adding a-cyanoacrylate and continuing to stir for one to two hours;

[0014] S5, mixing and stirring the products of S2 to S4 to obtain a coating protective glue;

[0015] S6, testing various properties of the coating protective glue;

[0016] S7, adjusting the raw material ratio according to the test results, and preparing the next round of preparation with the adjusted ratio.

[0017] Furthermore, the coating protective glue is made of the following raw materials in proportion by mass: 22 to 26 parts of liquid rubber material, 100 to 106 parts of xylene, 20 to 26 parts of waterproofing agent, 1 to 2 parts of α-hydroxybenzotriazole, 10 to 12 parts of loess, 35 to 39 parts of tackifier, 2 to 3 parts of initiator, 4 to 5 parts of isopropyl trititanate, 2 to 3 parts of zinc oxide and 7 to 8 parts of a-cyanoacrylate.

[0018] Furthermore, the liquid rubber material is EPDM rubber, the waterproofing agent includes 2 to 3 parts of polyethylene glycol acrylate, 6 to 8 parts of polyvinyl alcohol, and 12 to 14 parts of sepiolite powder in a mass ratio, the tackifier includes 32 to 35 parts of ethyl acetate and 3 to 4 parts of silane coupling agent in a mass ratio, and the initiator is tert-butyl perbenzoate.

[0019] Furthermore, the testing of various properties of the coating protective glue includes the following steps:

[0020] S61, extracting a protective glue sample from the produced coated protective glue;

[0021] S62, dropping 10 drops of the protective glue sample onto the first testing material continuously, recording the time required for the protective glue sample to completely dry, and obtaining the drying time of the protective glue sample;

[0022] S63, dropping 10 drops of the protective glue sample onto the second detection material continuously, covering the second detection material with the third detection material, and obtaining a bonded material after a time equal to the drying time;

[0023] S64, obtaining two or more bonded materials through the above steps, and performing various performance tests on the bonded materials and the protective adhesive contained therein;

[0024] S65, collecting performance test data, calculating various performance indicators of the protective glue according to the test data, and judging whether various performance indicators of the protective glue are qualified.

[0025] Furthermore, various performance tests on the bonded material and the protective adhesive contained therein include the following steps:

[0026] S641, taking any bonded material, shearing the protective glue contained in the bonded material at a constant speed by a shearing device, and recording the resistance encountered by the shearing device during the shearing process;

[0027] S642, taking any bonded material, pulling the bonded material apart in a direction perpendicular to the bonding surface at a constant speed until the bonded material is separated into two test materials, and recording the pulling force used in the pulling process;

[0028] S643, preparing a wooden container, wherein the bottom of the wooden container is provided with two or more holes, applying a portion of the protective adhesive sample on the top of the holes, and leaving it to stand for a time equal to the drying time;

[0029] S644, pour water into the container and record the humidity change at the bottom of the hole within a set time.

[0030] Furthermore, the calculation of the performance indicators of the protective adhesive includes the following steps:

[0031] S651, calculate the drying performance index of the protective glue according to the drying time;

[0032] S652, calculate the strength performance index of the protective glue according to the resistance of the shearing equipment;

[0033] S653, calculating the viscosity performance index of the protective glue according to the pulling force used in the pulling process;

[0034] S654, calculate the waterproof performance index of the protective glue according to the humidity change at the bottom of the hole.

[0035] Furthermore, when the raw material ratio is adjusted according to the test results, the adjusted raw materials include liquid rubber material, xylene, waterproofing agent and tackifier, and the raw material adjustment includes the following steps:

[0036] S71, obtaining the ratio of each raw material in the preparation and various performance indicators;

[0037] S72, judging whether the drying performance index is qualified, if not qualified, reducing the number of xylene by one, otherwise, maintaining the original ratio;

[0038] S73, judging whether the strength performance index is qualified, if not qualified, increasing the number of liquid rubber materials by one, otherwise, decreasing the number by one;

[0039] S74, judging whether the viscosity performance index is qualified, if not qualified, the number of tackifiers is increased by one, otherwise, the number is reduced by one;

[0040] S75, judging whether the waterproof performance index is qualified, if not qualified, the number of waterproofing agents is increased by one, otherwise, the number is reduced by one.

[0041] Furthermore, it also includes a preparation system for coating protective glue, including a production system and a detection system, the production system includes a storage module, a production container, a heating module and a stirring module, the storage module is used to store various raw materials for producing coating protective glue, the production container is used to contain various raw materials, the stirring module is used to stir the various raw materials in the production container, and the heating module is used to heat the production container;

[0042] The detection system includes an image detection module, a shearing device, a pulling device, a data acquisition module and a calculation module. The image detection module is used to determine whether the protective glue is completely dry through image detection. The shearing device is used to shear the protective glue. The pulling device is used to pull the bonded material bonded by the protective glue. The data acquisition module is used to collect various data generated during the detection process. The calculation module is used to calculate various indicators based on the various data collected by the data acquisition module.

[0043] The beneficial effects achieved by the present invention are:

[0044] 1. By setting various performance indicators to evaluate the performance of the protective glue, and obtaining various data of the protective glue through various tests, it is helpful to judge whether the performance of the produced protective glue is qualified, thereby avoiding the outflow of defective products.

[0045] 2. Adjusting the ratio of various raw materials according to whether various performance indicators are qualified is conducive to adjusting the raw material ratio according to actual conditions, avoiding excessive deviation between production results and expectations due to uneven raw material quality, and at the same time, minimizing raw material consumption when indicators are qualified. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The present invention can be further understood from the following description in conjunction with the accompanying drawings. The components in the figures are not necessarily drawn to scale, but the emphasis is placed on illustrating the principles of the embodiments. In different views, the same reference numerals designate the same parts.

[0047] Figure 1 It is a schematic diagram of the structure of the present invention.

[0048] Figure 2 It is the work flow chart of the present invention.

[0049] Figure 3 The present invention is a flow chart for testing various properties of the coating protective glue.

[0050] Figure 4 The present invention is a flow chart of performing various performance tests on the bonded material and the protective glue contained therein. DETAILED DESCRIPTION

[0051] The following is an explanation of the embodiments of the present invention through specific embodiments. Those skilled in the art can understand the advantages and effects of the present invention from the contents disclosed in this specification. The present invention can be implemented or applied through other different specific embodiments, and the details in this specification can also be modified and changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. In addition, the drawings of the present invention are only simple schematic illustrations and are not depicted according to actual sizes. It is stated in advance. The following embodiments will further explain the relevant technical contents of the present invention in detail, but the disclosed contents are not intended to limit the scope of protection of the present invention.

[0052] Embodiment 1: According to Figure 1 , Figure 2 , Figure 3 and Figure 4 This embodiment provides a method for preparing a coating protective glue with moisture-proof function, comprising the following steps:

[0053] S1, dissolving the liquid rubber material in xylene at room temperature and heating it to 70-80 degrees Celsius;

[0054] S2, add lubricant to the solution of S1 and stir for one to two hours, add α-hydroxybenzotriazole and stir for one to two hours;

[0055] S3, calcining the loess at 600-700 degrees Celsius, and grinding it into powder after cooling;

[0056] S4, heating the tackifier to 50-60 degrees Celsius, adding the initiator, waterproofing agent and zinc oxide, stirring for 30-40 minutes, and then adding a-cyanoacrylate and continuing to stir for one to two hours;

[0057] S5, mixing and stirring the products of S2 to S4 to obtain a coating protective glue;

[0058] S6, testing various properties of the coating protective glue;

[0059] S7, adjusting the raw material ratio according to the test results, and preparing the next round of preparation with the adjusted ratio.

[0060] Furthermore, the coating protective glue is made of the following raw materials in proportion by mass: 22 to 26 parts of liquid rubber material, 100 to 106 parts of xylene, 20 to 26 parts of waterproofing agent, 1 to 2 parts of α-hydroxybenzotriazole, 10 to 12 parts of loess, 35 to 39 parts of tackifier, 2 to 3 parts of initiator, 4 to 5 parts of isopropyl trititanate, 2 to 3 parts of zinc oxide and 7 to 8 parts of a-cyanoacrylate.

[0061] Furthermore, the liquid rubber material is EPDM rubber, the waterproofing agent includes 2 to 3 parts of polyethylene glycol acrylate, 6 to 8 parts of polyvinyl alcohol, and 12 to 14 parts of sepiolite powder in a mass ratio, the tackifier includes 32 to 35 parts of ethyl acetate and 3 to 4 parts of silane coupling agent in a mass ratio, and the initiator is tert-butyl perbenzoate.

[0062] Furthermore, the testing of various properties of the coating protective glue includes the following steps:

[0063] S61, extracting a protective glue sample from the produced coated protective glue;

[0064] S62, dropping 10 drops of the protective glue sample onto the first testing material continuously, recording the time required for the protective glue sample to completely dry, and obtaining the drying time of the protective glue sample;

[0065] S63, dropping 10 drops of the protective glue sample onto the second detection material continuously, covering the second detection material with the third detection material, and obtaining a bonded material after a time equal to the drying time;

[0066] S64, obtaining two or more bonded materials through the above steps, and performing various performance tests on the bonded materials and the protective adhesive contained therein;

[0067] S65, collecting performance test data, calculating various performance indicators of the protective glue according to the test data, and judging whether various performance indicators of the protective glue are qualified.

[0068] Furthermore, various performance tests on the bonded material and the protective adhesive contained therein include the following steps:

[0069] S641, taking any bonded material, shearing the protective glue contained in the bonded material at a constant speed by a shearing device, and recording the resistance encountered by the shearing device during the shearing process;

[0070] The resistance to the shearing device can be detected by a pressure sensor;

[0071] S642, taking any bonded material, pulling the bonded material apart in a direction perpendicular to the bonding surface at a constant speed until the bonded material is separated into two test materials, and recording the pulling force used in the pulling process;

[0072] S643, preparing a wooden container, wherein the bottom of the wooden container is provided with two or more holes, applying a portion of the protective adhesive sample on the top of the holes, and leaving it to stand for a time equal to the drying time;

[0073] S644, pour water into the container and record the humidity change at the bottom of the hole within a set time.

[0074] Specifically, the set time is set by those skilled in the art.

[0075] Furthermore, the calculation of the performance indicators of the protective adhesive includes the following steps:

[0076] S651, calculate the drying performance index of the protective glue according to the drying time;

[0077] The drying performance index can be calculated according to the following formula:

[0078]

[0079] Wherein, ZB1 is a drying performance index, which is used to characterize the drying speed of the protective glue. The larger the drying performance index, the faster the drying speed of the protective glue. V1 is the amount of the protective glue sample dripped onto the detection material. S1 is the surface area of ​​the protective glue sample dripped onto the detection material after it is completely dried. The surface area can be obtained through image recognition. t1 is the time required for the protective glue to completely dry from the beginning of dripping.

[0080] S652, calculate the strength performance index of the protective glue according to the resistance of the shearing equipment;

[0081] The strength performance index can be calculated according to the following formula:

[0082]

[0083] Among them, ZB2 is a strength performance index, which is used to characterize the strength of the protective glue. The larger the strength performance index, the higher the strength of the protective glue. 1maxis the maximum resistance encountered by the shearing device during the shearing process, t2 is the total time consumed in the shearing process, t3 is the time from the beginning of resistance detection to the beginning of resistance decrease, F1(t) is the resistance encountered during the shearing process, and A1(t) is the acceleration of the change of resistance encountered during the shearing process;

[0084] S653, calculating the viscosity performance index of the protective glue according to the pulling force used in the pulling process;

[0085] The viscosity performance index can be calculated according to the following formula:

[0086]

[0087] Wherein, ZB3 is a viscosity performance index, and the viscosity performance index is used to characterize the viscosity of the protective glue. The larger the viscosity performance index, the stronger the viscosity of the protective glue. 2max is the maximum pulling force used by the pulling device during the pulling process, t4 is the total time of the pulling process, t5 is the time from the beginning of detecting the pulling force to the beginning of the decrease of the pulling force, F2(t) is the pulling force used in the pulling process, and A2(t) is the acceleration of the change of the pulling force during the pulling process;

[0088] S654, calculate the waterproof performance index of the protective glue according to the humidity change at the bottom of the hole.

[0089] The waterproof performance index can be calculated according to the following formula:

[0090]

[0091] Wherein, ZB4 is a waterproof performance index, which is used to characterize the waterproof ability of the protective glue. The larger the waterproof performance index, the stronger the waterproof ability of the protective glue. I is the number of holes, S 2i is the hole area of ​​the ith hole, d i is the hole depth of the ith hole, t6 is the duration of the setting time, RH i (t) is the humidity at the opening of the i-th hole toward the outside of the container.

[0092] Specifically, each performance indicator has a corresponding set threshold value. When a performance indicator is greater than the corresponding set threshold value, the performance is considered qualified. The set threshold value is determined by a technician in this field who conducts experiments on existing coating protective glue and obtains the corresponding performance indicators, and is set with reference to the performance indicators. The set time can be set according to the penetration rate of water in wood. The greater the penetration rate, the shorter the set time. The set time can generally be set to 20 to 30 minutes.

[0093] Furthermore, when the raw material ratio is adjusted according to the test results, the adjusted raw materials include liquid rubber material, xylene, waterproofing agent and tackifier, and the raw material adjustment includes the following steps:

[0094] S71, obtaining the ratio of each raw material in the preparation and various performance indicators;

[0095] S72, judging whether the drying performance index is qualified, if not qualified, reducing the number of xylene by one, otherwise, maintaining the original ratio;

[0096] Specifically, if the number of portions after the ratio adjustment exceeds the ratio stated above, the adjustment of the raw material will be cancelled;

[0097] S73, judging whether the strength performance index is qualified, if not qualified, increasing the number of liquid rubber materials by one, otherwise, decreasing the number by one;

[0098] S74, judging whether the viscosity performance index is qualified, if not qualified, the number of tackifiers is increased by one, otherwise, the number is reduced by one;

[0099] S75, judging whether the waterproof performance index is qualified, if not qualified, the number of waterproofing agents is increased by one, otherwise, the number is reduced by one.

[0100] Furthermore, it also includes a preparation system for coating protective glue, including a production system and a detection system, the production system includes a storage module, a production container, a heating module and a stirring module, the storage module is used to store various raw materials for producing coating protective glue, the production container is used to contain various raw materials, the stirring module is used to stir the various raw materials in the production container, and the heating module is used to heat the production container;

[0101] The detection system includes an image detection module, a shearing device, a pulling device, a data acquisition module and a calculation module. The image detection module is used to determine whether the protective glue is completely dry through image detection. Specifically, it can be determined by image detection whether the protective glue sample adheres to the glass rod. If there is no wire drawing between the protective glue sample and the glass rod when they are separated, it is considered to be completely dry. The shearing device is used to shear the protective glue, and the pulling device is used to pull the bonded material bonded by the protective glue. The data acquisition module is used to collect various data generated during the detection process, and the calculation module is used to calculate various indicators based on the various data collected by the data acquisition module.

[0102] The beneficial effects of this solution are as follows: 1. By setting various performance indicators to evaluate the various properties of the protective glue and obtaining various data of the protective glue through various tests, it is helpful to judge whether the various properties of the produced protective glue are qualified, thereby avoiding the outflow of defective products.

[0103] 2. Adjusting the ratio of various raw materials according to whether various performance indicators are qualified is conducive to adjusting the raw material ratio according to actual conditions, avoiding excessive deviation between production results and expectations due to uneven raw material quality, and at the same time, minimizing raw material consumption when indicators are qualified.

[0104] Embodiment 2: This embodiment should be understood to include all the features of any of the above embodiments, and further improves on the basis thereof, and also includes a method for controlling the stirring speed of the stirring module, comprising the following steps:

[0105] 1. The stirring module stirs at the initial setting speed;

[0106] 2. Detect the resistance encountered by the stirring part of the stirring module during the stirring process;

[0107] 3. Obtain the stirring speed adjusted by the stirring module according to the following formula;

[0108]

[0109] Wherein, speed2 is the adjusted stirring speed, speed1 is the initial speed when the stirring module stirs various raw materials, L1 is the length of the stirring module immersed in the liquid part of the production container during the first stirring, F3 is the resistance encountered by the stirring part when the stirring module continuously stirs in clean water at the initial speed, L0 is the length of the stirring part immersed in the liquid part of the production container when the stirring module stirs in clean water at the initial speed, and F4(L) is the resistance encountered by the part of the stirring module immersed in the production container during the first stirring;

[0110] 4. Adjust the stirring speed according to the adjusted stirring speed obtained, and return to step 2.

[0111] The beneficial effects of this embodiment are as follows: the stirring speed is adjusted according to the resistance encountered by the stirring part during the stirring process, which is conducive to appropriately reducing the stirring speed when the resistance is large and appropriately increasing the stirring speed when the resistance is small, thereby avoiding equipment damage caused by high-speed stirring when the resistance is large. By automatically adjusting the stirring speed, it is conducive to improving the degree of automation of the equipment.

[0112] The above disclosed contents are only preferred feasible embodiments of the present invention, and do not limit the protection scope of the present invention. Therefore, all equivalent technical changes made by using the contents of the present invention specification and drawings are included in the protection scope of the present invention. In addition, the elements therein can be updated with the development of technology. The above units are only examples. Those skilled in the art can use corresponding units according to different designs according to actual needs when implementing this solution.

Claims

1. A method for preparing a coating protective adhesive with moisture-proof function, It is characterized in that The following steps are involved: S1, dissolving the liquid rubber material in xylene at room temperature and heating it to 70-80 degrees Celsius; S2, add lubricant to the solution of S1 and stir for one to two hours, add α-hydroxybenzotriazole and stir for one to two hours; S3, calcining the loess at 600-700 degrees Celsius, and grinding it into powder after cooling; S4, heating the tackifier to 50-60 degrees Celsius, adding the initiator, waterproofing agent and zinc oxide, stirring for 30-40 minutes, and then adding a-cyanoacrylate and continuing to stir for one to two hours; S5, mixing and stirring the products of S2 to S4 to obtain a coating protective glue; S6, testing various properties of the coating protective glue; S7, adjusting the raw material ratio according to the test results, and preparing the next round of preparation with the adjusted ratio.

2. A method for preparing a coating protective adhesive with moisture-proof function according to claim 1, It is characterized in that The coating protective glue is made of the following raw materials in proportion by mass: 22-26 parts of liquid rubber material, 100-106 parts of xylene, 20-26 parts of waterproofing agent, 1-2 parts of α-hydroxybenzotriazole, 10-12 parts of loess, 35-39 parts of tackifier, 2-3 parts of initiator, 4-5 parts of isopropyl trititanate, 2-3 parts of zinc oxide and 7-8 parts of a-cyanoacrylate.

3. A method for preparing a coating protective adhesive with moisture-proof function according to claim 2, It is characterized in that The liquid rubber material is EPDM rubber, the waterproofing agent includes 2-3 parts of polyethylene glycol acrylate, 6-8 parts of polyvinyl alcohol, and 12-14 parts of sepiolite powder in a mass ratio, the tackifier includes 32-35 parts of ethyl acetate and 3-4 parts of silane coupling agent in a mass ratio, and the initiator is tert-butyl perbenzoate.

4. The method for preparing a coating protective adhesive with moisture-proof function according to claim 3, It is characterized in that Testing the various properties of the coating protective glue includes the following steps: S61, extracting a protective glue sample from the produced coated protective glue; S62, dropping 10 drops of the protective glue sample onto the first testing material continuously, recording the time required for the protective glue sample to completely dry, and obtaining the drying time of the protective glue sample; S63, dropping 10 drops of the protective glue sample onto the second detection material continuously, covering the second detection material with the third detection material, and obtaining a bonded material after a time equal to the drying time; S64, obtaining two or more bonded materials through the above steps, and performing various performance tests on the bonded materials and the protective adhesive contained therein; S65, collecting performance test data, calculating various performance indicators of the protective glue according to the test data, and judging whether various performance indicators of the protective glue are qualified.

5. A method for preparing a coating protective adhesive with moisture-proof function according to claim 4, It is characterized in that The various performance tests of the bonded materials and the protective adhesives they contain include the following steps: S641, taking any bonded material, shearing the protective glue contained in the bonded material at a constant speed by a shearing device, and recording the resistance encountered by the shearing device during the shearing process; S642, taking any bonded material, pulling the bonded material apart in a direction perpendicular to the bonding surface at a constant speed until the bonded material is separated into two test materials, and recording the pulling force used in the pulling process; S643, preparing a wooden container, wherein the bottom of the wooden container is provided with two or more holes, applying a portion of the protective adhesive sample on the top of the holes, and leaving it to stand for a time equal to the drying time; S644, pour water into the container and record the humidity change at the bottom of the hole within a set time.

6. A method for preparing a coating protective adhesive with moisture-proof function according to claim 5, It is characterized in that Calculating the performance indicators of the protective glue includes the following steps: S651, calculate the drying performance index of the protective glue according to the drying time; S652, calculate the strength performance index of the protective glue according to the resistance of the shearing equipment; S653, calculating the viscosity performance index of the protective glue according to the pulling force used in the pulling process; S654, calculate the waterproof performance index of the protective glue according to the humidity change at the bottom of the hole.

7. A method for preparing a coating protective adhesive with moisture-proof function according to claim 6, It is characterized in that When adjusting the raw material ratio according to the test results, the adjusted raw materials include liquid rubber material, xylene, waterproofing agent and tackifier, and adjusting the raw materials includes the following steps: S71, obtaining the ratio of each raw material in the preparation and various performance indicators; S72, judging whether the drying performance index is qualified, if not qualified, reducing the number of xylene by one, otherwise, maintaining the original ratio; S73, judging whether the strength performance index is qualified, if not qualified, increasing the number of liquid rubber materials by one, otherwise, decreasing the number by one; S74, judging whether the viscosity performance index is qualified, if not qualified, the number of tackifiers is increased by one, otherwise, the number is reduced by one; S75, judging whether the waterproof performance index is qualified, if not qualified, the number of waterproofing agents is increased by one, otherwise, the number is reduced by one.

8. The method for preparing a coating protective adhesive with moisture-proof function according to claim 7, It is characterized in that Also included is a preparation system for coating protective glue, including a production system and a detection system, the production system including a storage module, a production container, a heating module and a stirring module, the storage module is used to store various raw materials for producing coating protective glue, the production container is used to contain various raw materials, the stirring module is used to stir the various raw materials in the production container, and the heating module is used to heat the production container; The detection system includes an image detection module, a shearing device, a pulling device, a data acquisition module and a calculation module. The image detection module is used to determine whether the protective glue is completely dry through image detection. The shearing device is used to shear the protective glue. The pulling device is used to pull the bonded material bonded by the protective glue. The data acquisition module is used to collect various data generated during the detection process. The calculation module is used to calculate various indicators based on the various data collected by the data acquisition module.

Citation Information

Patent Citations

  • Waterproof EPDM (Ethylene-Propylene-Diene Monomer) glue and preparation method thereof

    CN103254846A

  • Cold-pressing glue, preparation method and application of cold-pressing glue

    CN107384258A

  • Method for testing and evaluating water resistance of waterproof material

    CN111189721A

  • Detection technological process for semi-finished products and finished products of semiconductor cutting mucosa-reducing films

    CN114113468A

  • Method for making a high solids interactive coating composition and ink jet recording medium

    US20020055552A1