Moisture-curable polyurethane hot melt adhesive and preparation method thereof
By using liquid polyester polyols, crystalline polyester polyols and other components in the wet-cured polyurethane hot melt adhesive, combined with high-temperature dehydration and vacuum stirring technology, the problem of insufficient fluidity of the wet-cured polyurethane hot melt adhesive is solved, and the problem of insufficient fluidity of the wet-cured polyurethane hot melt adhesive is achieved. Good coating uniformity and initial viscosity.
Patent Information
- Application Number
- CN202411187923.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-03
AI Technical Summary
The existing wet cured polyurethane hot melt adhesives are not fluid enough during actual use, resulting in poor coating uniformity.
采用包括液体聚酯多元醇、结晶性聚酯多元醇、共聚丙烯酸树脂、异氰酸酯、流平剂和添加剂的湿固化聚氨酯热熔胶,通过高温脱水、真空搅拌和氮气保护等步骤制备,提升流动性和黏度稳定性。
Ensure good wetting during construction and initial viscosity under high-temperature construction conditions, and improve the fluidity and coating uniformity of wet-cured polyurethane hot melt adhesive.
Smart Images

Figure CN119060674A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hot melt adhesive preparation, and in particular to a moisture-curing polyurethane hot melt adhesive and a preparation method thereof. Background Art
[0002] Moisture-curing polyurethane hot melt adhesives are mostly made by reacting polyester and / or polyether polyols with diisocyanates (MDI, TDI, HDI, etc.) to generate polyurethane prepolymers with -NCO end-capping. The isocyanate groups in the system react with substances containing active hydroxyl groups inside or outside the system to generate polyurethane groups or polyureas, thereby improving the strength of the system and achieving the purpose of efficient bonding.
[0003] However, the existing moisture-curing polyurethane hot melt adhesive has less than ideal fluidity during actual use, resulting in poor coating uniformity. Summary of the invention
[0004] The purpose of the present invention is to provide a moisture-curing polyurethane hot melt adhesive and a preparation method thereof, so as to solve the problem that the moisture-curing polyurethane hot melt adhesive in the prior art has poor fluidity during actual use, resulting in poor coating uniformity.
[0005] To achieve the above-mentioned object, the present invention provides a moisture-curing polyurethane hot melt adhesive, which comprises the following components in parts by weight: 5-15 parts of liquid polyester polyol, 15-30 parts of crystalline polyester polyol, 50-70 parts of copolymerized acrylic resin, 10-15 parts of isocyanate, 0.1-0.5 parts of leveling agent and additives, wherein the additives are composed of 0.4-0.6 parts of stannous octoate, 0.5-1.5 parts of chain extender, 2-3 parts of bismorpholinyl diethyl ether and 2-3 parts of inorganic acid.
[0006] The present invention also provides a method for preparing a moisture-curing polyurethane hot melt adhesive, which is applied to the moisture-curing polyurethane hot melt adhesive as described above, comprising the following steps:
[0007] S1, adding liquid polyester polyol, crystalline polyester polyol and copolymerized acrylic resin into a reaction kettle, mixing, and performing high-temperature dehydration treatment to obtain a treatment liquid;
[0008] S2. When the water content in the reactor is reduced to less than 100 ppm, the treated liquid is cooled under a nitrogen atmosphere, a leveling agent is added to the interior of the reactor, and the mixture is stirred and mixed under a vacuum degree of <100 Pa;
[0009] S3, raising the temperature of the treatment liquid in the reactor to 80-100°C, adding isocyanate and stannous octoate, and stirring the reaction under the condition of vacuum degree <100Pa;
[0010] S4, after the isocyanate and stannous octoate react with the treatment liquid in the reactor, a chain extender is added to react;
[0011] S5. After the chain extender reaction is completed, the reactor is heated, bismorpholinyl diethyl ether and inorganic acid are added, and stirred and mixed under the condition of vacuum degree <100 Pa;
[0012] S6. Nitrogen is injected into the reactor, and the material is quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then put into an oven for aging to obtain a moisture-curing polyurethane hot melt adhesive.
[0013] Wherein, in step S1, the high temperature dehydration temperature is 125-135°C, and the high temperature dehydration time is 2 hours.
[0014] Wherein, in step S2, the cooling temperature of the treatment liquid is 65-75°C, and the stirring and mixing time in the reactor is 15 minutes.
[0015] Wherein, in step S3, the stirring reaction time in the reactor is 60 minutes.
[0016] Wherein, in step S4, the reaction conditions of the chain extender are: the reaction temperature of the reactor is between 85° C. and 95° C., the vacuum degree of the reactor is less than 100 Pa, and the reaction time is 120 min.
[0017] Wherein, in step S5, the heating temperature of the reactor is 130° C., and the stirring and mixing time in the reactor is 25 min.
[0018] Wherein, in step S6, the drying temperature of the drying box is 65-75°C.
[0019] The invention discloses a moisture-curing polyurethane hot melt adhesive and a preparation method thereof, comprising a liquid polyester polyol, a crystalline polyester polyol, a copolymerized acrylic resin, an isocyanate, a leveling agent and an additive. The aliphatic part in the liquid polyester polyol provides the system with good fluidity to ensure good wetting during the construction process. The crystalline polyester polyol plays a role of rapid crystallization, so that the adhesive can be quickly strengthened under high-temperature construction conditions and generate a high initial adhesion. In addition, by adding a certain amount of the leveling agent, the viscosity stability of the polyurethane hot melt adhesive system is improved, so that the moisture-curing polyurethane hot melt adhesive has the characteristics of low flow melt temperature, good fluidity and uniform coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0021] Figure 1 It is a flow chart of the steps of the method for preparing the moisture-curing polyurethane hot melt adhesive in the first embodiment provided by the present invention.
[0022] Figure 2 It is a flow chart of the steps of the method for preparing moisture-curing polyurethane hot melt adhesive in the second embodiment provided by the present invention.
[0023] Figure 3 It is a flow chart of the steps of the method for preparing moisture-curing polyurethane hot melt adhesive in the third embodiment provided by the present invention. DETAILED DESCRIPTION
[0024] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0025] The invention provides a moisture-curing polyurethane hot melt adhesive. The moisture-curing polyurethane hot melt adhesive comprises the following components in parts by weight: 5-15 parts of liquid polyester polyol, 15-30 parts of crystalline polyester polyol, 50-70 parts of copolymerized acrylic resin, 10-15 parts of isocyanate, 0.1-0.5 parts of leveling agent and additives, wherein the additives are composed of 0.4-0.6 parts of stannous octoate, 0.5-1.5 parts of chain extender, 2-3 parts of bismorpholinyl diethyl ether and 2-3 parts of inorganic acid.
[0026] Wherein, the liquid polyester polyol includes at least one temperature-sensitive polyester polyol.
[0027] In this embodiment, the aliphatic part in the liquid polyester polyol provides good fluidity for the system, ensuring good infiltration during the construction process, and the crystalline polyester polyol plays a role of rapid crystallization, so that the adhesive can quickly strengthen under high-temperature construction conditions and produce a higher initial adhesion. In addition, since the liquid polyester polyol includes at least one thermosensitive polyester polyol, the use of thermosensitive polyester polyol can ensure that the product can be used under low temperature conditions, and by adding a certain amount of leveling agent, the stability of the viscosity of the polyurethane hot melt adhesive system is improved, so that the moisture-curing polyurethane hot melt adhesive has the characteristics of low flow melt temperature, good fluidity and uniform coating.
[0028] Example 1, please refer to Figure 1 The present invention also provides a method for preparing a moisture-curing polyurethane hot melt adhesive, which is applied to the moisture-curing polyurethane hot melt adhesive as described above, comprising the following steps:
[0029] S101: adding 5 parts of liquid polyester polyol, 15 parts of crystalline polyester polyol and 50 parts of copolymerized acrylic resin into a reaction kettle and mixing them, and performing high temperature dehydration treatment at a high temperature dehydration temperature of 125° C. for 2 hours to obtain a treatment liquid;
[0030] S102: When the water in the reactor is removed to below 100 ppm, the treated liquid is cooled to 65° C. under a nitrogen atmosphere, a leveling agent is added to the interior of the reactor, and the mixture is stirred and mixed for 15 minutes under a vacuum degree of <100 Pa;
[0031] S103: raising the temperature of the treatment liquid in the reaction kettle to 80° C., adding 10 parts of isocyanate and 0.4 parts of stannous octoate, and stirring the reaction for 60 minutes under the condition of vacuum degree <100 Pa;
[0032] S104: After the isocyanate and stannous octoate react with the treatment liquid in the reactor, 0.5 parts of a chain extender are added, and the reaction is carried out under the conditions of a reaction temperature of 85° C., a vacuum degree of the reactor of less than 100 Pa, and a reaction time of 120 min;
[0033] S105: After the chain extender reaction is completed, the temperature in the reactor is raised to 130° C., 2 parts of bismorpholinyl diethyl ether and 2 parts of inorganic acid are added, and the mixture is stirred and mixed for 25 minutes under a vacuum degree of <100 Pa;
[0034] S106: nitrogen is injected into the reactor, and the material is quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then placed in an oven for aging at a drying temperature of 65° C. to obtain a moisture-curable polyurethane hot melt adhesive.
[0035] In this embodiment, first, 5 parts of liquid polyester polyol, 15 parts of crystalline polyester polyol and 50 parts of copolymerized acrylic resin are added to a reactor and mixed, and high-temperature dehydration treatment is performed under the conditions of a high-temperature dehydration temperature of 125°C and a high-temperature dehydration time of 2 hours to obtain a treatment liquid, and then when the water in the reactor is removed to less than 100 ppm, the treatment liquid is cooled to 65°C under a nitrogen atmosphere, a leveling agent is added to the inside of the reactor, and the mixture is stirred for 15 minutes under a vacuum degree of <100Pa, and then the temperature of the treatment liquid in the reactor is raised to 80°C, 10 parts of isocyanate and 0.4 parts of stannous octoate are added, and the mixture is stirred for 15 minutes under a vacuum degree of <100Pa. The mixture was stirred and reacted for 60 minutes. After the isocyanate and stannous octoate reacted with the treatment liquid in the reactor, 0.5 parts of a chain extender were added, and the reaction temperature was 85°C, the vacuum degree of the reactor was <100Pa, and the reaction time was 120 minutes. After the reaction of the chain extender was completed, the temperature in the reactor was raised to 130°C, 2 parts of dimorpholinyl diethyl ether and 2 parts of an inorganic acid were added, and the mixture was stirred and mixed for 25 minutes under the condition of a vacuum degree <100Pa. Finally, nitrogen was flushed into the reactor, the material was quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then added to an oven for aging at a drying temperature of 65°C to obtain a moisture-curing polyurethane hot melt adhesive.
[0036] Example 2, please refer to Figure 2 The present invention also provides a method for preparing a moisture-curing polyurethane hot melt adhesive, which is applied to the moisture-curing polyurethane hot melt adhesive as described above, comprising the following steps:
[0037] S201: adding 15 parts of liquid polyester polyol, 30 parts of crystalline polyester polyol and 70 parts of copolymerized acrylic resin into a reaction kettle and mixing them, and performing high temperature dehydration treatment at a high temperature dehydration temperature of 135° C. for 2 hours to obtain a treatment liquid;
[0038] S202: When the water content in the reactor is reduced to less than 100 ppm, the treated liquid is cooled to 75° C. under a nitrogen atmosphere, 0.5 parts of a leveling agent is added to the reactor, and the mixture is stirred and mixed for 15 minutes under a vacuum degree of <100 Pa;
[0039] S203: raising the temperature of the treatment liquid in the reaction kettle to 100° C., adding 15 parts of isocyanate and 0.6 parts of stannous octoate, and stirring the reaction for 60 minutes under the condition of vacuum degree <100 Pa;
[0040] S204: After the isocyanate and stannous octoate react with the treatment liquid in the reactor, 1.5 parts of a chain extender are added, and the reaction is carried out under the conditions of a reaction temperature of 95° C., a vacuum degree of the reactor of less than 100 Pa, and a reaction time of 120 min;
[0041] S205: After the chain extender reaction is completed, the temperature in the reactor is raised to 130° C., 3 parts of bismorpholinyl diethyl ether and 3 parts of inorganic acid are added, and the mixture is stirred and mixed for 25 minutes under the condition of vacuum degree <100 Pa;
[0042] S206: nitrogen is injected into the reactor, and the material is quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then placed in an oven for aging at a drying temperature of 75° C. to obtain a moisture-curable polyurethane hot melt adhesive.
[0043] In this embodiment, 15 parts of liquid polyester polyol, 30 parts of crystalline polyester polyol and 70 parts of copolymerized acrylic resin are first added to a reactor and mixed, and high-temperature dehydration treatment is performed under the conditions of a high-temperature dehydration temperature of 135°C and a high-temperature dehydration time of 2 hours to obtain a treatment liquid, and then when the water in the reactor is removed to less than 100 ppm, the treatment liquid is cooled to 75°C under a nitrogen atmosphere, 0.5 leveling agent is added to the inside of the reactor, and the mixture is stirred for 15 minutes under a vacuum degree of <100Pa, and then the temperature of the treatment liquid in the reactor is raised to 100°C, 15 parts of isocyanate and 0.6 parts of stannous octoate are added, and the mixture is stirred for 15 minutes under a vacuum degree of <100Pa. The mixture was stirred and reacted for 60 minutes under the condition of , after the isocyanate and stannous octoate completed the reaction with the treatment liquid in the reactor, 0.5 parts of a chain extender were added, and the reaction was carried out under the conditions of a reaction temperature of 95°C, a vacuum degree of the reactor of less than 100Pa, and a reaction time of 120min. After the reaction of the chain extender was completed, the temperature in the reactor was raised to 130°C, 3 parts of dimorpholinyl diethyl ether and 3 parts of an inorganic acid were added, and the mixture was stirred and mixed for 25 minutes under the condition of a vacuum degree of less than 100Pa. Finally, nitrogen was flushed into the reactor, the material was quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then added to an oven for aging at a drying temperature of 75°C to obtain a moisture-curing polyurethane hot melt adhesive.
[0044] Example 3, please refer to Figure 3 The present invention also provides a method for preparing a moisture-curing polyurethane hot melt adhesive, which is applied to the moisture-curing polyurethane hot melt adhesive as described above, comprising the following steps:
[0045] S301: adding 10 parts of liquid polyester polyol, 22.5 parts of crystalline polyester polyol and 60 parts of copolymerized acrylic resin into a reaction kettle and mixing them, and performing high temperature dehydration treatment at a high temperature dehydration temperature of 130° C. for a high temperature dehydration time of 2 hours to obtain a treatment liquid;
[0046] S302: When the water content in the reactor is reduced to less than 100 ppm, the treated liquid is cooled to 70° C. under a nitrogen atmosphere, 0.3 parts of a leveling agent is added to the reactor, and the mixture is stirred and mixed for 15 minutes under a vacuum degree of <100 Pa;
[0047] S303: raising the temperature of the treatment liquid in the reaction kettle to 90° C., adding 13 parts of isocyanate and 0.5 parts of stannous octoate, and stirring the reaction for 60 minutes under the condition of vacuum degree <100 Pa;
[0048] S304: After the isocyanate and stannous octoate react with the treatment liquid in the reactor, 1 part of a chain extender is added, and the reaction is carried out under the conditions of a reaction temperature of 90° C., a vacuum degree of the reactor of less than 100 Pa, and a reaction time of 120 min;
[0049] S305: After the chain extender reaction is completed, the temperature in the reactor is raised to 130° C., 2.5 parts of bismorpholinyl diethyl ether and 2.5 parts of inorganic acid are added, and stirred and mixed for 25 minutes under the condition of vacuum degree <100 Pa;
[0050] S306: nitrogen is injected into the reactor, the material is quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then put into an oven for aging at a drying temperature of 70° C. to obtain a moisture-curing polyurethane hot melt adhesive.
[0051] In this embodiment, first, 10 parts of liquid polyester polyol, 22.5 parts of crystalline polyester polyol and 60 parts of copolymerized acrylic resin are added to a reactor and mixed, and high-temperature dehydration treatment is performed under the conditions of a high-temperature dehydration temperature of 130°C and a high-temperature dehydration time of 2 hours to obtain a treatment liquid, and then when the water in the reactor is removed to less than 100 ppm, the treatment liquid is cooled to 70°C under a nitrogen atmosphere, 0.3 parts of a leveling agent are added to the inside of the reactor, and the mixture is stirred for 15 minutes under a vacuum degree of <100Pa, and then the temperature of the treatment liquid in the reactor is raised to 90°C, 13 parts of isocyanate and 0.5 parts of stannous octoate are added, and the mixture is stirred for 15 minutes under a vacuum degree of <100Pa. The mixture was stirred and reacted for 60 minutes under the condition of 100 Pa. After the isocyanate and stannous octoate reacted with the treatment liquid in the reactor, 1 part of a chain extender was added, and the reaction was carried out under the conditions of a reaction temperature of 90° C., a vacuum degree of the reactor of less than 100 Pa, and a reaction time of 120 minutes. After the reaction of the chain extender was completed, the temperature in the reactor was raised to 130° C., 2.5 parts of dimorpholinyl diethyl ether and 2.5 parts of an inorganic acid were added, and the mixture was stirred and mixed for 25 minutes under the condition of a vacuum degree of less than 100 Pa. Finally, nitrogen was flushed into the reactor, the material was quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then added to an oven for aging at a drying temperature of 70° C. to obtain a moisture-curing polyurethane hot melt adhesive.
[0052] What is disclosed above is only a preferred embodiment of the present invention, and it certainly cannot be used to limit the scope of rights of the present invention. Ordinary technicians in this field can understand that all or part of the processes of the above embodiment and equivalent changes made according to the claims of the present invention still fall within the scope of the invention.
Claims
1. A moisture-curing polyurethane hot melt adhesive, characterized in that: It includes the following components in parts by weight: 5-15 parts of liquid polyester polyol, 15-30 parts of crystalline polyester polyol, 50-70 parts of copolymerized acrylic resin, 10-15 parts of isocyanate, 0.1-0.5 parts of leveling agent and additives, wherein the additives are composed of 0.4-0.6 parts of stannous octoate, 0.5-1.5 parts of chain extender, 2-3 parts of bismorpholinyl diethyl ether and 2-3 parts of inorganic acid.
2. A method for preparing a moisture-curing polyurethane hot melt adhesive, applied to the moisture-curing polyurethane hot melt adhesive as claimed in claim 1, characterized in that: The steps include: S1, adding liquid polyester polyol, crystalline polyester polyol and copolymerized acrylic resin into a reaction kettle, mixing, and performing high-temperature dehydration treatment to obtain a treatment liquid; S2. When the water content in the reactor is reduced to less than 100 ppm, the treated liquid is cooled under a nitrogen atmosphere, a leveling agent is added to the interior of the reactor, and the mixture is stirred and mixed under a vacuum degree of <100 Pa; S3, raising the temperature of the treatment liquid in the reactor to 80-100°C, adding isocyanate and stannous octoate, and stirring the reaction under the condition of vacuum degree <100Pa; S4, after the isocyanate and stannous octoate react with the treatment liquid in the reactor, a chain extender is added to react; S5. After the chain extender reaction is completed, the reactor is heated, bismorpholinyl diethyl ether and inorganic acid are added, and stirred and mixed under the condition of vacuum degree <100 Pa; S6. Nitrogen is injected into the reactor, and the material is quickly discharged under the protection of nitrogen and packaged in an aluminum foil bag, and then put into an oven for aging to obtain a moisture-curing polyurethane hot melt adhesive.
3. The method for preparing a moisture-curable polyurethane hot melt adhesive according to claim 2, characterized in that: In step S1, the high temperature dehydration temperature is 125-135°C, and the high temperature dehydration time is 2 hours.
4. The moisture-curable polyurethane hot melt adhesive and the preparation method thereof according to claim 3, characterized in that: In step S2, the cooling temperature of the treatment liquid is 65-75°C, and the stirring and mixing time in the reactor is 15 minutes.
5. The method for preparing a moisture-curable polyurethane hot melt adhesive according to claim 4, characterized in that: In step S3, the stirring reaction time in the reactor is 60 minutes.
6. The method for preparing a moisture-curable polyurethane hot melt adhesive according to claim 5, characterized in that: In step S4, the reaction conditions of the chain extender are: the reaction temperature of the reactor is between 85° C. and 95° C., the vacuum degree of the reactor is less than 100 Pa, and the reaction time is 120 min.
7. The method for preparing a moisture-curable polyurethane hot melt adhesive according to claim 6, characterized in that: In step S5, the heating temperature of the reactor is 130°C, and the stirring and mixing time in the reactor is 25 minutes.
8. The method for preparing a moisture-curable polyurethane hot melt adhesive according to claim 7, characterized in that: In step S6, the drying temperature of the drying box is 65-75°C.