Pressure-sensitive adhesive with excellent weather resistance, preparation method of pressure-sensitive adhesive and polaroid
By adjusting components and structures, solvent-free pressure-sensitive adhesives formed in the crosslinking network solve the problem of the polarizer's adhesion increasing with time, stable adhesion and weather resistance, extend the service life of the polarizer, and Reduces environmental pollution and energy consumption.
Patent Information
- Application Number
- CN202411323833.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-12-03
AI Technical Summary
The longer the existing polarizer pressure-sensitive adhesive is stored, the more adhesion the force increases, resulting in cohesion damage, and problems such as floating, lifting, and bubbles, affecting service life.
Using solvent-free pressure-sensitive adhesive, by adjusting the weight ratio of hydroxy UV monomer to crosslinking agent and the number of functional groups, combined with acrylic polyurethane prepolymer, UV hard monomer, UV soft monomer, unsaturated acid and isocyanate compounds. The crosslinking network structure is formed to increase the cohesion of the adhesive layer and inhibit the growth of adhesion, and coat and cure using ultraviolet curing technology.
The pressure-sensitive adhesive has excellent weather resistance and stable peeling force. The peeling force grows slowly after 12 months at room temperature, avoiding adverse phenomena such as floating and bubbles, extending the service life of the polarizer, and reducing environmental pollution and Energy consumption.
Smart Images

Figure CN119060682A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a pressure-sensitive adhesive with excellent weather resistance and a preparation method thereof, and a polarizer, belonging to the technical field of polarizers. Background Art
[0002] Polarizer is an optical device used to polarize natural light or light of any polarization to a specific direction. The basic structure of the polarizer includes a PVA layer (polyvinyl alcohol layer) in the middle and two protective layers arranged on both sides of the PVA layer, of which the PVA layer plays a polarizing role. However, since PVA is very easy to hydrolyze and is easily affected by the external environment, in order to protect the physical properties of the polarizing film, a layer of optical film with high light transmittance, good water resistance and certain mechanical strength is generally compounded on both sides of the PVA layer for protection, thus forming the original polarizer. According to different usage requirements, a certain thickness of pressure sensitive adhesive (PSA) is coated on one side of the original polarizer, and a release film is compounded to protect the PSA; and a protective film is compounded on the other side to obtain a semi-finished polarizer. The semi-finished polarizer is then stripped and cut into sheets for edge grinding to obtain a finished polarizer.
[0003] The existing polarizer PSA line production process contains a large amount of solvents, and a drying process is required after coating, which consumes a lot of electricity and increases carbon emissions. At the same time, the volatile organic solvents need to be RTO-burned after collection, which consumes energy and increases carbon emissions. The use of UV-curable pressure-sensitive adhesive can overcome the above-mentioned shortcomings of solvent-based pressure-sensitive adhesive and eliminate the PSA drying process. For example, Chinese patent 2024106940512 discloses a polarizer containing UV-curable PSA glue and a preparation method thereof, comprising a PVA layer, an outer inner protective layer and an inner inner protective layer bonded to the upper and lower surfaces of the PVA layer by UV glue, a protective film on the surface of the outer inner protective layer, and a release film adhered to the surface of the inner inner protective layer by a pressure-sensitive adhesive layer; the coating liquid of the pressure-sensitive adhesive layer comprises the following components in parts by weight: 40 to 70 parts by weight of a polymer prepolymer, 10 to 30 parts by weight of a cross-linking agent A; 10 to 30 parts by weight of a cross-linking agent B, 0.05 to 0.3 parts by weight of a photoinitiator, 1 to 5 parts by weight of a coupling agent, 1 to 5 parts by weight of an antistatic agent and 10 to 20 parts by weight of a diluent. The invention solves the problem of imbalance between the existing PSA adhesive viscosity and adhesive properties (such as peeling force, cohesion, re-stickability, etc.). The PSA adhesive layer has excellent cohesion without residual adhesive, good re-stickability, and a peeling force of 200-1000gf / 25mm; and the adhesive system is solvent-free and environmentally friendly.
[0004] However, when the pressure-sensitive adhesive is used for polarizers, there is a common problem that the adhesion becomes significantly larger with the storage time, and sometimes cohesive failure (such as floating, warping, bubbles, etc.) occurs during weather resistance testing. Therefore, how to improve the weather resistance of the existing polarizer pressure-sensitive adhesive system and extend its service life has become a problem that needs to be solved urgently. Summary of the invention
[0005] The present invention overcomes the drawbacks of the prior art and provides a pressure-sensitive adhesive with excellent weather resistance and a preparation method thereof, as well as a polarizer. The pressure-sensitive adhesive is solvent-free and environmentally friendly, and after online coating and lamination, only the release film surface needs to be subjected to ultraviolet irradiation before winding.
[0006] The technical solution adopted by the present invention to solve its technical problem is:
[0007] A pressure-sensitive adhesive with excellent weather resistance, comprising the following components in parts by weight:
[0008]
[0009] The present invention further comprises: the weight ratio of the hydroxyl UV monomer to the crosslinking agent is 1:1 to 3:1, and the molar number of the hydroxyl functional group in the hydroxyl UV monomer is in excess of the molar number of the isocyanate functional group in the crosslinking agent.
[0010] The present invention further comprises: the weight average molecular weight of the acrylic polyurethane prepolymer is 10,000 to 80,000; the UV hard monomer is a multifunctional acrylate or a multifunctional methacrylate; the photoinitiator is a free radical photoinitiator; the crosslinking agent is an isocyanate compound; the coupling agent is a silane coupling agent; and the antistatic agent is an ionic liquid antistatic agent.
[0011] Preferably, the acrylic polyurethane prepolymer is selected from UF-C051 of Kyoeisha Co., Ltd., UA-1138P of Shin-Nakamura Co., Ltd., DR-U299 of Changxing Materials Co., Ltd., DR-U282 of Changxing Materials Co., Ltd. (molecular weight 20,000-30,000), CN9178NS and CN9014NS of Sartomer Co.;
[0012] Preferably, the UV hard monomer is any one or more of diacrylate, dimethacrylate, triacrylate, trimethacrylate;
[0013] Preferably, the UV soft monomer is any one or more of tetrahydrofuran acrylate, isooctyl acrylate, butyl acrylate, and ethyl acrylate;
[0014] Preferably, the unsaturated acid is any one or more of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, 4-(3-(acryloyloxy)propoxy)benzoic acid, and crotonic acid;
[0015] Preferably, the hydroxyl UV monomer is selected from any one or more of 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 6-hydroxyhexyl acrylate, 6-hydroxyhexyl methacrylate, 8-hydroxyoctyl acrylate, 8-hydroxyoctyl methacrylate, 8-hydroxyoctyl acrylate, 8-hydroxyoctyl methacrylate, 6-hydroxyhexyl acrylate, 6-hydroxyhexyl methacrylate, 2-hydroxyethylene glycol acrylate, 2-hydroxyethylene glycol methacrylate, 2-hydroxypropylene glycol acrylate, and 2-hydroxypropylene glycol methacrylate;
[0016] Preferably, the photoinitiator is any one or more of 184 photoinitiator, 907 photoinitiator, 1173 photoinitiator, benzophenone, 127 photoinitiator and 2959 photoinitiator;
[0017] Preferably, the cross-linking agent is any one or more of butylene diisocyanate, hexamethylene diisocyanate, cyclopentylene diisocyanate, tetramethylene diisocyanate, isophorone diisocyanate, and tetramethylxylene diisocyanate;
[0018] Preferably, the coupling agent is any one of KH550, KH560, KH570, A151, A171 and A172;
[0019] Preferably, the antistatic agent is FC4400 from 3M.
[0020] The gel fraction of the pressure-sensitive adhesive after UV curing is 82% to 88%, the initial peeling force on the glass is 200 to 500 gf / 25 mm, and after one year at room temperature, the peeling force on the glass is 300 to 600 gf / 25 mm.
[0021] The method for preparing the pressure-sensitive adhesive with excellent weather resistance comprises the following steps:
[0022] S1. Mix UV hard monomer, UV soft monomer, unsaturated acid, and hydroxyl UV monomer evenly, add coupling agent, antistatic agent, and crosslinking agent, and stir evenly; then add photoinitiator, and stir until dissolved evenly to obtain a mixed solution a;
[0023] S2. Add the mixed solution a into the acrylic polyurethane prepolymer, stir and mix evenly, and obtain the pressure-sensitive adhesive solution after defoaming, which can be directly used for coating.
[0024] The preparation process and storage environment of the pressure-sensitive adhesive must be protected from light; the prepared adhesive solution must be used within 48 hours.
[0025] A polarizer comprises a PVA layer, an outer protective layer and an inner protective layer adhered to the upper and lower surfaces of the PVA layer by UV adhesive, a release film is adhered to the outer side of the inner protective layer by a pressure-sensitive adhesive layer, and a protective film is arranged on the outer side of the outer protective layer; the pressure-sensitive adhesive layer is a pressure-sensitive adhesive with excellent weather resistance.
[0026] The thickness of the pressure-sensitive adhesive layer (6) is 10 to 30 μm, and the surface resistance is 9.9×10 11 Ω / □ or less.
[0027] The UV curing lamp source used for curing the pressure-sensitive adhesive layer (6) is a high-pressure mercury lamp or a halogen lamp, and the UVA curing energy is 1000 mj / cm 2 Above, the light intensity of UVA is 300mw / cm 2 above.
[0028] The beneficial effects of the present invention are:
[0029] The present invention provides a pressure-sensitive adhesive with excellent weather resistance and a preparation method thereof, with excellent cohesion and no residual adhesive, and a peeling force that increases slowly over time at room temperature (23±3°C), and has good adhesion and weather resistance. The initial adhesion of the pressure-sensitive adhesive to glass is 200-500gf / 25mm, and the re-adhesion is good; the peeling force to glass increases slowly over 12 months at room temperature, and can reach 300-600gf / 25mm, with a small increase. After 12 months at room temperature, the sheet is tested for glass weather resistance for 500h without bubbles, edge warping, floating, and white spots, which solves the problem that the peeling force of the existing UV-PSA adhesive increases over time at room temperature and is not easy to peel off.
[0030] The present invention contains four monomers, namely, acrylic polyurethane prepolymer, UV hard monomer, UV soft monomer, unsaturated acid, and hydroxyl UV monomer. The UV hard monomer, UV soft monomer, unsaturated acid, and hydroxyl UV monomer react with acrylic polyurethane prepolymer to form a cross-linked network. The UV hard monomer and acrylic polyurethane prepolymer form the main structure of the cross-linked network, and the UV soft monomer, UV hard monomer, and acrylic polyurethane prepolymer form the secondary structure of the cross-linked network, so that the glue has viscoelasticity; a small amount of isocyanate compound is dispersed in the three-dimensional network structure, which acts as a stress dispersion point during UV curing to reduce the deformation and warping of the colloid caused by volume shrinkage, the unsaturated acid double bond is grafted onto the main glue molecular chain to enhance the bonding force with the bonded surface, and the hydroxyl UV monomer double bond is grafted onto the main glue molecular chain to enhance the bonding force between the hydroxyl layer and the bonded surface, thereby ensuring the bonding effect. During the later curing, the hydroxyl group and the isocyanate cross-linking agent gradually undergo a slow cross-linking reaction, further enhancing the cohesive force and inhibiting the growth of the bonding force to the adherend. The combined effect of the components of the present invention enables the finished product of the pressure-sensitive adhesive to have high adhesion after UV curing, and during storage, the small molecular components in the adhesive layer system are not easy to precipitate, ensuring that the adhesion increases slowly.
[0031] The main reason why the peeling force of existing UV-PSA adhesive increases over time at room temperature is that the molecular weight of the pressure-sensitive adhesive is too small, which leads to a decrease in cohesive strength over a long period of time. The migration of low molecular weight free monomers and low polymerization degree molecules enhances the wettability of the adhered surface and increases the anchoring force with the adherend. When the anchoring force is greater than the cohesive force of the adhesive layer itself, floating and poor bubbles are likely to occur. The present invention increases the molecular weight of the adhesive through the reasonable allocation of component types and their amounts, controls the gel fraction of the pressure-sensitive adhesive after UV curing at a high level of 82% to 88%, and improves the cohesive force of the adhesive layer itself. At the same time, through the gradual slow cross-linking reaction between the hydroxyl UV monomer and the isocyanate cross-linking agent, the attraction to low molecular weight free monomers and low polymerization degree molecules is increased to prevent them from migrating to the adhered surface, thereby avoiding the increase of anchoring force. The present invention increases the cohesive force of the adhesive layer itself and suppresses the anchoring force with the adherend, thereby ensuring that the bonding force of the adhesive layer is at a relatively stable level for a long time and has good weather resistance.
[0032] The pressure-sensitive adhesive used in the present invention is a solvent-free type, which has excellent application and gelling properties. The use of solvent-free UV-curing PSA adhesive reduces VOC emissions, is environmentally friendly, and saves energy and reduces emissions. Compared with heat-curing PSA adhesive, the pressure-sensitive adhesive of the present invention does not require drying and aging, and cures quickly at room temperature, thereby improving production efficiency, reducing energy consumption and product turnover time.
[0033] The present invention also provides a polarizer, which uses a pressure-sensitive adhesive with excellent weather resistance as the adhesion layer between the inner protective layer and the release film. The peeling force on the glass increases slowly after one year at room temperature, and the weather resistance is excellent after one year of storage, thereby extending the shelf life of the finished polarizer and reducing the risk of inventory scrapping due to slow sales. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the structure of the polarizer of the present invention;
[0035] In the figure: 1. PVA layer; 2. UV adhesive layer; 3. outer inner protective layer; 4. inner inner protective layer; 5. protective film; 6. pressure-sensitive adhesive layer; 7. release film. DETAILED DESCRIPTION
[0036] The present invention is described in detail below with reference to the accompanying drawings.
[0037] The directions or their approximate terms described throughout the present invention, such as "front", "rear", "left", "right", "up (top)", "down (bottom)", "inside", "outside", "side", etc., are mainly used with reference to the directions of the accompanying drawings. Each direction or its approximate terms are only used to assist in the explanation and understanding of the embodiments of the present invention, and are not used to limit the present invention.
[0038] A pressure-sensitive adhesive with excellent weather resistance, comprising the following components in parts by weight:
[0039]
[0040] Preferably include the following components in parts by weight:
[0041]
[0042]
[0043] The acrylic polyurethane prepolymer has a weight average molecular weight of 10,000 to 80,000, preferably 12,000 to 72,000, and can be selected from: UF-C051 of Kyoeisha Co., Ltd., UA-1138P of Shin-Nakamura Co., Ltd., DR-U299 of Changxing Materials Co., Ltd., DR-U282 of Changxing Materials Co., Ltd. (molecular weight 20,000-30,000), CN9178NS and CN9014NS of Sartomer Co., Ltd.
[0044] The UV hard monomer is a multifunctional acrylate or a multifunctional methacrylate, such as any one or more of diacrylate, dimethacrylate, triacrylate, and trimethacrylate; further preferably, it is one or more of diethylene glycol diacrylate (DEGDA), triethylene glycol diacrylate (TEGDA), 1,6-hexanediol diacrylate (HDDA), neopentyl glycol diacrylate (NPGDA), glycidyl methacrylate (GMA), polyethylene glycol diacrylate, pentaerythritol triacrylate, and trimethylolpropane triacrylate (TMPTA).
[0045] The UV soft monomer is selected from any one or more of tetrahydrofuran acrylate, isooctyl acrylate, butyl acrylate, and ethyl acrylate.
[0046] The unsaturated acid is selected from any one or more of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, 4-(3-(acryloyloxy)propoxy)benzoic acid, and crotonic acid.
[0047] The hydroxy UV monomer is selected from any one or more of 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 6-hydroxyhexyl acrylate, 6-hydroxyhexyl methacrylate, 8-hydroxyoctyl acrylate, 8-hydroxyoctyl methacrylate, 8-hydroxyoctyl acrylate, 8-hydroxyoctyl methacrylate, 6-hydroxyhexyl acrylate, 6-hydroxyhexyl methacrylate, 2-hydroxyethylene glycol acrylate, 2-hydroxyethylene glycol methacrylate, 2-hydroxypropylene glycol acrylate, and 2-hydroxypropylene glycol methacrylate. Further preferred is any one or more of 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethylene glycol acrylate, 2-hydroxyethylene glycol methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, and 4-hydroxybutyl methacrylate.
[0048] The photoinitiator is a free radical photoinitiator, preferably any one or more of 184 photoinitiator, 907 photoinitiator, 1173 photoinitiator, benzophenone, 127 photoinitiator and 2959 photoinitiator.
[0049] The crosslinking agent is an isocyanate compound, preferably any one or more selected from butylene diisocyanate, hexamethylene diisocyanate, cyclopentylene diisocyanate, tetramethylene diisocyanate, isophorone diisocyanate, and tetramethylxylylene diisocyanate.
[0050] The coupling agent is a silane coupling agent, preferably any one selected from KH550, KH560, KH570, A151, A171 and A172;
[0051] The antistatic agent is an ionic liquid antistatic agent, preferably FC4400 from 3M.
[0052] It should be emphasized that, based on the above weight components, the weight ratio of the hydroxyl UV monomer to the crosslinking agent is 1:1 to 3:1, preferably 2:1, which can not only ensure the crosslinking degree of the slow reaction in the later stage, but also avoid the excessive isocyanate compound causing poor precipitation. At the same time, the ratio of the two must also satisfy the requirement that the molar number of the hydroxyl functional group is in excess of the molar number of the isocyanate functional group, preferably the ratio of the molar number of the hydroxyl functional group to the molar number of the isocyanate functional group is (1.1 to 1.6): 1. Since the hydroxyl UV monomer and the crosslinking agent isocyanate compound will undergo a slow crosslinking reaction, the molar ratio of the functional groups of the two is very important. In order to ensure the crosslinking system generated later in the adhesive layer, it is required that the molar number of the hydroxyl functional group in the hydroxyl UV monomer is controlled to the molar number of the isocyanate functional group in the crosslinking agent at (1.1 to 1.6): 1. If the molar number of hydroxyl functional groups in the hydroxyl UV monomer is too small, there is a risk of precipitation after the isocyanate reaction is excessive and stored for a long time; if the molar number of hydroxyl functional groups in the hydroxyl UV monomer is too large, the subsequent cross-linked network structure will be small and have poor support, which cannot meet the effective attraction of low molecular weight free monomers and low polymerization degree molecules. Therefore, the weight ratio of the hydroxyl UV monomer to the cross-linking agent is 3:1 to 1:1, and at the same time, the molar number of hydroxyl functional groups is excessive to the molar number of isocyanate functional groups, which can effectively control the network structure state generated by the subsequent cross-linking reaction, ensure its effective attraction to low molecular weight free monomers and low polymerization degree molecules, and avoid their migration.
[0053] The gel fraction of the pressure-sensitive adhesive after UV curing is controlled at 82% to 88%. A higher gel fraction is beneficial to increasing the initial adhesion of the adhesive layer and can also reduce the migration of low molecular weight free monomers and low polymerization degree molecules to the surface of the adhesive layer to a certain extent.
[0054] The pressure-sensitive adhesive disclosed by the present invention does not contain solvent, is environmentally friendly, has excellent applicability, has moderate adhesive force, good re-stickability and firm bonding, has no warping, peeling and bubble defects in aging resistance test, has a slow increase in adhesive force at room temperature (23±3°C) within one year of storage, has a gel fraction of 82% to 88% after UV PSA adhesive is cured, has excellent cohesive force and can be peeled without residual adhesive, has an initial adhesive force to glass of 200 to 500 gf / 25mm, and has a slow increase in peeling force to glass at room temperature after one year of storage, which is controlled at 300 to 600 gf / 25mm.
[0055] A method for preparing a pressure-sensitive adhesive with excellent weather resistance comprises the following steps:
[0056] S1. Mix UV hard monomer, UV soft monomer, unsaturated acid, and hydroxyl UV monomer evenly, add coupling agent, antistatic agent, and crosslinking agent, and stir evenly; then add photoinitiator, and stir until dissolved evenly to obtain a mixed solution a;
[0057] S2. Add the mixed solution a into the acrylic polyurethane prepolymer, stir and mix evenly, and obtain the pressure-sensitive adhesive solution after defoaming, which can be directly used for coating.
[0058] It should be noted that: 1. The preparation process and storage environment of the pressure-sensitive adhesive must be protected from light; 2. The prepared adhesive must be used within 48 hours, otherwise its performance will be affected.
[0059] A polarizer, comprising a PVA layer 1, an outer protective layer 3 and an inner protective layer 4 attached to the upper and lower surfaces of the PVA layer 1 by UV adhesive 2, a release film 7 adhered to the outer side of the inner protective layer 4 by a pressure-sensitive adhesive layer 6, and a protective film 5 is arranged on the outer side of the outer protective layer 3. The pressure-sensitive adhesive layer 6 adopts the pressure-sensitive adhesive of the present invention.
[0060] In the above polarizer, the thickness of the pressure-sensitive adhesive layer is 10 to 30 μm, and the surface resistance is 9.9×10 11 Ω / □ or less.
[0061] In the above polarizer, according to the different functions of the product, the outer protective layer can be selected from one of TAC, PMMA, and PET films, and the inner protective layer can be selected from one of TAC, PMMA, and COP films. A functional layer, such as AG, HC, or LR layer, can also be included between the outer protective layer and the protective film; if the functional layer has good wear resistance and hardness, the outer side of the functional layer may not require a protective film.
[0062] The method for preparing the polarizer comprises the following steps:
[0063] S1. Unwind the PVA original film at the first unwinding position, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain PVA polarized film; adhere inner protective layers to the upper and lower surfaces of the PVA polarized film respectively by UV glue, the outer side being the outer inner protective layer, and the inner side being the inner inner protective layer;
[0064] S2, unwinding the release film at the second unwinding position, coating it with pressure-sensitive adhesive, laminating it to the inner protective layer, and curing it under UV light, with the irradiated surface being the release film surface;
[0065] S3, unwinding the protective film at the third unwinding position, laminating it to the outer inner protective layer, and rewinding it to obtain a semi-finished polarizer;
[0066] S4, the semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0067] In the method for preparing the polarizer, in S2, the pressure-sensitive adhesive may be coated on the surface of the inner protective layer, and then attached to the release surface of the release film.
[0068] In the preparation method of the polarizer, the UV curing lamp source in S2 is preferably a high pressure mercury lamp or a halogen lamp, and the UVA curing energy is 1000 mj / cm 2 Above, the light intensity of UVA is 300mw / cm 2 above.
[0069] In the preparation method of the polarizer, the UV lamp irradiation is incident on the release film surface or the release film surface and the original reverse surface. Double-sided incidence requires actual adjustment of curing energy and light intensity to ensure sufficient curing and avoid deformation and decomposition of polarizers due to heat.
[0070] See also Figure 1 The polarizer layer structure of the present invention is sequentially provided with a protective film 5, an outer protective layer 3, a UV adhesive 2, a PVA layer 1, a UV adhesive 2, an inner protective layer 4, a pressure-sensitive adhesive layer 6 and a release film 7 from top to bottom. The preparation process includes the following steps:
[0071] S1. Unwind the PVA original film at the first unwinding position, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain PVA polarized film; adhere inner protective layers to the upper and lower surfaces of the PVA polarized film respectively by UV glue, the outer layer is the outer inner protective layer, and the layer coated with PSA glue is the inner inner protective layer;
[0072] S2, unwind the release film at the second unwinding position, apply UV PSA glue, adhere it to the inner protective layer, and cure it under UV light, with the irradiated surface being the release film surface;
[0073] S3, unwinding the protective film at the third unwinding position, laminating it to the outer inner protective layer, and rewinding it to obtain a semi-finished polarizer;
[0074] S4, the semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0075] The present invention will be further described below in conjunction with the embodiments.
[0076] In the following examples, except for the manufacturers and brands specified, other raw materials are commercially available products and are chemically pure.
[0077] Example 1
[0078] A pressure-sensitive adhesive with excellent weather resistance, specifically composed of:
[0079]
[0080] The preparation process of the above pressure-sensitive adhesive is:
[0081] S1. In a dark environment, mix all monomers except the main agent UF-C051 evenly, add coupling agent KH560, antistatic agent FC4400, and hexamethylene diisocyanate and stir evenly, then add initiator 907 and stir until dissolved evenly to obtain a mixed solution a;
[0082] S2. Add the mixed solution a to the main agent UF-C051, stir and mix evenly, defoam to obtain the finished pressure-sensitive adhesive, and keep it away from light for later use.
[0083] A method for preparing a polarizer, comprising the following steps:
[0084] S1. Unwind the PVA original film at the first unwinding position, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain PVA polarizers; adhere PMMA and PMMA inner protective layers to the upper and lower surfaces of the PVA polarizers respectively by UV glue, the outer layer is the outer layer, and the PSA adhesive layer is the inner layer;
[0085] S2, unwinding the release film at the second unwinding place, coating the prepared pressure-sensitive adhesive, laminating the inner PMMA inner protective layer after S1, and curing it by UV irradiation, with the irradiated surface being the release film surface;
[0086] S3, unwinding the PET protective film at the third unwinding position, laminating the outer inner protective layer passing through S2, and rewinding to obtain a semi-finished polarizer;
[0087] S4, the upper semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0088] The preparation method of the upper polarizer, wherein the UV curing in S2 uses a high pressure mercury lamp UVA curing energy of 1000mj / cm 2 , UVA light intensity is 350mw / cm 2 .
[0089] Example 2
[0090] A pressure-sensitive adhesive with excellent weather resistance, specifically composed of:
[0091]
[0092] The preparation process of the above pressure-sensitive adhesive is:
[0093] S1. In a dark environment, mix all monomers except the main agent DR-U299 evenly, add coupling agent KH550, antistatic agent FC4400, isophorone diisocyanate and stir evenly, then add initiator 907 and stir until dissolved evenly to obtain a mixed solution a;
[0094] S2. Add the mixed solution a to the DR-U299 main agent, stir and mix evenly, defoam to obtain the finished pressure-sensitive adhesive, and keep it away from light for later use.
[0095] A method for preparing a polarizer, comprising the following steps:
[0096] S1. Unwind the PVA original film at the first unwinding place, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain a polarized film; adhere PMMA and COP inner protective layers to the upper and lower surfaces of the polarized film respectively by UV glue, the outer layer is the outer layer, and the PSA adhesive layer is the inner layer;
[0097] S2, unwinding the release film at the second unwinding place, coating the prepared pressure-sensitive adhesive, laminating the inner COP inner protective layer after S1, and curing it by UV irradiation, with the irradiated surface being the release film surface;
[0098] S3, unwinding the PET protective film at the third unwinding position, laminating the outer inner protective layer passing through S2, and rewinding to obtain a semi-finished polarizer;
[0099] S4, the upper semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0100] The preparation method of the upper polarizer, wherein the energy of the UVA curing high pressure mercury lamp in S2 is 1100 mj / cm 2 , UVA light intensity is 420mw / cm 2 .
[0101] Example 3
[0102] A pressure-sensitive adhesive with excellent weather resistance, specifically composed of:
[0103]
[0104]
[0105] The preparation process of the above pressure-sensitive adhesive is:
[0106] S1. In the dark, mix all monomers except the main agent UA-1138P evenly, add coupling agent A171, antistatic agent FC4400, butylene diisocyanate and stir evenly, then add initiator 184 and stir until dissolved evenly to obtain a mixed solution a;
[0107] S2. Add the mixed solution a to the UA-1138P main agent, stir and mix evenly, defoam to obtain the finished pressure-sensitive adhesive, and keep it away from light for standby use.
[0108] A method for preparing a polarizer, comprising the following steps:
[0109] S1. Unwind the PVA original film at the first unwinding position, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain a polarized film; adhere PMMA and PMMA inner protective layers to the upper and lower surfaces of the polarized film respectively by UV glue, the outer layer is the outer layer, and the PSA adhesive layer is the inner layer;
[0110] S2, unwinding the release film at the second unwinding place, coating the prepared pressure-sensitive adhesive, laminating the inner PMMA protective layer after S1, and curing it by UV irradiation, with the irradiated surface being the release film surface;
[0111] S3, unwinding the PET protective film at the third unwinding position, laminating the outer inner protective layer passing through S2, and rewinding to obtain a semi-finished polarizer;
[0112] S4, the upper semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0113] The preparation method of the upper polarizer, wherein the energy of the UVA curing lamp in S2 is 1000 mj / cm 2 , UVA light intensity is 380mw / cm 2 .
[0114] Example 4
[0115] A pressure-sensitive adhesive with excellent weather resistance, specifically composed of:
[0116]
[0117]
[0118] The preparation process of the above pressure-sensitive adhesive is:
[0119] S1. In the dark, mix all monomers except the main agent CN9178NS evenly, add coupling agent KH560, antistatic agent FC4400, butylene diisocyanate and stir evenly, then add 907 initiator and stir until dissolved evenly to obtain mixed solution a;
[0120] S2. Add the mixed solution a to the CN9178NS main agent, stir and mix evenly, defoam to obtain the pressure-sensitive adhesive, and keep it away from light for later use.
[0121] A method for preparing a polarizer, comprising the following steps:
[0122] S1. Unwind the PVA original film at the first unwinding position, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain a polarized film; adhere PET and TAC inner protective layers to the upper and lower surfaces of the polarized film respectively through UV glue, the outer layer is the outer layer, and the PSA adhesive layer is the inner layer;
[0123] S2, unwinding the release film at the second unwinding place, coating the prepared pressure-sensitive adhesive, laminating the inner TAC inner protective layer after S1, and curing it through UV irradiation, with the irradiated surface being the release film surface;
[0124] S3, unwinding the PET protective film at the third unwinding position, laminating the outer inner protective layer passing through S2, and rewinding to obtain a semi-finished polarizer;
[0125] S4, the upper semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0126] The preparation method of the upper polarizer, wherein the energy of the UVA curing lamp in S2 is 1200 mj / cm 2 , UVA light intensity is 440mw / cm 2 .
[0127] Comparative Example 1
[0128] This comparative example adopts the formula and preparation method of Example 1 of the specification of Chinese Patent 2024106940512, and the specific composition of the solvent-free UV PSA adhesive is as follows:
[0129]
[0130] The preparation process of the above pressure-sensitive adhesive is:
[0131] Mix all monomers except the main agent UF-C051 evenly, add coupling agent and antistatic agent and stir evenly, then add 907 initiator and stir until dissolved evenly to obtain mixed solution a;
[0132] Add the mixed solution a into the main agent UF-C051, stir and mix evenly, and defoam to obtain the finished UV PSA adhesive for standby use.
[0133] The above preparation and storage environment should be protected from light.
[0134] A method for preparing a polarizer, comprising the following steps:
[0135] S1. Unwind the PVA original film at the first unwinding position, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain PVA polarizers; adhere PMMA and PMMA inner protective layers to the upper and lower surfaces of the PVA polarizers respectively by UV glue, the outer layer is the outer layer, and the PSA adhesive layer is the inner layer;
[0136] S2, unwinding the release film at the second unwinding place, coating the prepared UV PSA glue, laminating the inner PMMA inner protective layer after S1, and curing it by UV irradiation, with the irradiated surface being the release film surface;
[0137] S3, unwinding the PET protective film at the third unwinding position, laminating the outer inner protective layer passing through S2, and rewinding to obtain a semi-finished polarizer;
[0138] S4, the upper semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0139] The preparation method of the upper polarizer, wherein the UV curing in S2 uses a high pressure mercury lamp UVA curing energy of 1000mj / cm 2 , UVA light intensity is 200mw / cm 2 .
[0140] Comparative Example 2
[0141] The commercially available UV PSA manufacturer Fujikura Chemical brand LKG-2110 (CN) was used, and the initiator and coupling agent were added according to the manufacturer's recommendations. The mixture was stirred and mixed evenly, and the finished UV PSA glue was defoamed to obtain a standby.
[0142] The above preparation and storage environment should be protected from light.
[0143] A method for preparing a polarizer, comprising the following steps:
[0144] S1. Unwind the PVA original film at the first unwinding place, and perform swelling, dyeing, bridging, stretching, washing, fixing and drying to obtain a polarized film; adhere PMMA and COP inner protective layers to the upper and lower surfaces of the polarized film respectively by UV glue, the outer layer is the outer layer, and the PSA adhesive layer is the inner layer;
[0145] S2, unwind the release film at the second unwinding location, apply UV PSA glue, adhere to the inner COP protective layer that has passed through S1, and cure it through UV irradiation, with the irradiated surface being the release film surface;
[0146] S3, unwinding the PET protective film at the third unwinding position, laminating the outer inner protective layer passing through S2, and rewinding to obtain a semi-finished polarizer;
[0147] S4, the upper semi-finished polarizer is unwound on the cutting line, and is cut and edge-grinded to obtain a finished polarizer sheet.
[0148] The preparation method of the upper polarizer, wherein the energy of the UVA curing high pressure mercury lamp in S2 is 1100 mj / cm 2 , UVA light intensity is 220mw / cm 2 .
[0149] The following comparative examples 3 to 14 are all comparative examples of Example 1.
[0150] Comparative Example 3
[0151] Based on Example 1, the unsaturated acid acrylic acid was removed, and the other components, contents and preparation methods remained unchanged.
[0152] Comparative Example 4
[0153] On the basis of Example 1, the hydroxyl UV monomer 2-hydroxyethyl acrylate was removed, and the other components, contents and preparation methods remained unchanged.
[0154] Comparative Example 5
[0155] Based on Example 1, the cross-linking agent hexamethylene diisocyanate was removed, and the other components, contents and preparation methods remained unchanged.
[0156] Comparative Example 6
[0157] Based on Example 1, 3-(4-methoxybenzoyl) acrylic acid (outside the types specified in the present invention) is used as the unsaturated acid, and the other components, contents and preparation methods remain unchanged.
[0158] Comparative Example 7
[0159] On the basis of Example 1, the amount of acrylic acid was increased to 12 parts by weight (exceeding the upper limit of the amount of unsaturated acid), and the other components, contents and preparation methods remained unchanged.
[0160] Comparative Example 8
[0161] On the basis of Example 1, the amount of acrylic acid was reduced to 4 parts by weight (exceeding the lower limit of the amount of unsaturated acid), and the other components, contents and preparation methods remained unchanged.
[0162] Comparative Example 9
[0163] On the basis of Example 1, the amount of 2-hydroxyethyl acrylate was increased to 21 parts by weight (exceeding the upper limit of the amount of hydroxyl UV monomer), and the other components, contents and preparation methods remained unchanged.
[0164] Comparative Example 10
[0165] On the basis of Example 1, the amount of 2-hydroxyethyl acrylate was reduced to 9 parts by weight (exceeding the lower limit of the amount of hydroxyl UV monomer), and the other components, contents and preparation methods remained unchanged.
[0166] Comparative Example 11
[0167] On the basis of Example 1, the amount of hexamethylene diisocyanate was increased to 11 parts by weight (exceeding the upper limit of the amount of the cross-linking agent), and the other components, contents and preparation methods remained unchanged.
[0168] Comparative Example 12
[0169] On the basis of Example 1, the amount of hexamethylene diisocyanate was reduced to 4 parts by weight (exceeding the lower limit of the amount of the cross-linking agent), and the other components, contents and preparation methods remained unchanged.
[0170] Comparative Example 13
[0171] On the basis of Example 1, the amount of UF-C051 was increased to 72 parts by weight (exceeding the upper limit of the amount of acrylic polyurethane prepolymer), and the other components, contents and preparation methods remained unchanged.
[0172] Comparative Example 14
[0173] Based on Example 1, the amount of UF-C051 was reduced to 28 parts by weight (exceeding the lower limit of the amount of acrylic polyurethane prepolymer), and the other components, contents and preparation methods remained unchanged.
[0174] Embodiment 15
[0175] On the basis of Example 1, the amount of 2-hydroxyethyl acrylate was increased to 20 parts by weight, and the components, contents, preparation methods of other pressure-sensitive adhesives, and the structure and preparation methods of polarizers remained unchanged.
[0176] At this time, the weight ratio of 2-hydroxyethyl acrylate to hexamethylene diisocyanate is 20:6, which is out of the range of 1:1 to 3:1.
[0177] Comparative Example 16
[0178] On the basis of Example 1, the amount of the cross-linking agent hexamethylene diisocyanate was increased to 10 parts by weight, and the other components, contents, preparation methods of the pressure-sensitive adhesive, and the structure and preparation methods of the polarizer remained unchanged.
[0179] At this time, 2-hydroxyethyl acrylate and hexamethylene diisocyanate are both 10 parts by weight, and the weight ratio is 1:1, which meets the weight ratio range limit requirements of the two. The ratio of the molar amount of the hydroxyl functional group in 2-hydroxyethyl acrylate (M116.08) to the molar amount of the isocyanate functional group in hexamethylene diisocyanate (M168.19) is 0.724:1, and the hexamethylene diisocyanate is in excess.
[0180] The pressure-sensitive adhesive products prepared in Examples 1 to 4 and Comparative Examples 1 to 16 were tested for performance. The items and standards of the performance tests are as follows:
[0181] 1. Peeling force test: Take a sample with a width of 25mm and a length of about 150mm, prepare a smooth surface of soda glass, wipe it clean with a dust-free cloth slightly dipped in ethanol, let it stand for 30 minutes, stick the sample on the glass, roll the sample back and forth three times with a 2kg roller at a speed of 10±0.5mm / s, let it stand for 24 hours at a temperature of 23±2℃ and a relative humidity of 50±5%, peel it 180° at a speed of 300mm / min, record the value, and measure the sample three times in parallel.
[0182] 2. Cohesion test: Take a sample with a width of 25mm and a length of about 150mm, prepare a smooth surface of sodium glass, wipe it clean with a dust-free cloth slightly dipped in ethanol, let it stand for 30 minutes, stick a sample with an area of 25mm×25mm on the glass, use a 2kg roller to roll the prepared sample back and forth three times at a speed of 10±0.5mm / s, fold the other free end of the sample in half and let the adhesive surface self-adhere, and hang a 1kg weight on the free end, place it in an oven at 80℃ and bake it for 1h. After taking the sample out of the oven, let it stand for 15min, record the sliding distance, and measure the sample three times in parallel.
[0183] 3. Weather resistance test: high temperature 80℃, high temperature and humidity 60℃, 90%RH, cold -35℃, hot and cold shock -35~80℃.
[0184] 4. Gel fraction: Weigh 1.1242-0.1250g of glue and put it into an analytical balance, record the weight as m1, put it into a bottle, add 20g of ethyl acetate into the bottle, tighten the bottle cap and soak for 12 hours, put it into an oscillator and shake for 15 minutes, take a 10cm*10cm 200-mesh stainless steel filter and weigh it as m2, immediately introduce the shaken glue into the filter, wash the bottle once and then introduce it into the filter to avoid residue, let it stand for 30 minutes, put it into an 80℃ oven for 3 hours, take it out and weigh the total weight as m3, then the formula for calculating the gel fraction is: [(m3-m2) / m1]*100%.
[0185] The test results are as follows:
[0186] Table 1 Performance test table of polarizer PSA prepared in Examples and Comparative Examples
[0187]
[0188]
[0189] Table 2 Performance test table of polarizer PSA prepared in Examples and Comparative Examples when stored at room temperature for 1 year
[0190]
[0191]
[0192]
[0193] It can be seen from the data in the table that the UV PSA adhesive prepared in Examples 1 to 4 has good applicability, moderate peeling force at day 0, no residual adhesive, and good re-adhesion; after 1 year at room temperature, the peeling force does not exceed 550g / 25mm, and the growth rate is small. The sheet is tested for 500h in weather resistance to glass without bubbles, edge warping, floating, white spots, etc.
[0194] Comparative Examples 1 and 2 are existing pressure-sensitive adhesives, which are compared with the product of the present invention. It can be seen from the data in Comparative Example 1 that Comparative Example 1 is a solvent-free UV PSA adhesive previously developed by our company, with excellent applicability, 180° peeling force of 220gf / 25mm at 0 days, and no residual glue; the 180° peeling force at room temperature after 1 year increased significantly, reaching 820gf / 25mm. Although there are still no peeling force residual glue and warping, the increase in peeling force is obvious, which significantly increases the risk of rework. Comparative Example 2 is an existing commercially available UV PSA, with a large initial peeling force and residual glue; the 180° peeling force at room temperature after 1 year increased significantly, reaching 1410gf / 25mm, and the weather resistance test showed edge warping and bubble defects.
[0195] Comparative Examples 3 to 5 are set for the main components in the adhesive system of the present invention. Comparative Example 3 removes the unsaturated acid, resulting in poor adhesive application, low initial peeling force, a gel fraction of 78%, poor cohesion, weight drop, and edge warping in the weather resistance test. Comparative Example 4 removes the hydroxyl UV monomer. The hydroxyl UV monomer can reduce the viscosity of the adhesive and make up for the initial bonding force. Its absence leads to poor adhesive application, low initial peeling force, a gel fraction of 77%, and poor cohesion. In addition, the hydroxyl UV monomer is also used for the post-curing reaction with the isocyanate compound. After its absence, the post-curing of the adhesive layer cannot be achieved, and the peeling force increases significantly. The 180° peeling force at room temperature after 1 year reaches 865gf / 25mm, which significantly increases the risk of rework. In Comparative Example 5, the isocyanate cross-linking agent is removed. The isocyanate cross-linking agent does not react in the early stage, but will slowly react with the hydroxyl UV monomer after long-term storage to increase the cohesive strength and resist the diffusion of small molecules. When the adhesive system lacks the isocyanate cross-linking agent, the initial 0-day peeling force meets the requirements, but the 180° peeling force at room temperature after 1 year increases significantly to 980gf / 25mm, which proves that the cohesive strength of the adhesive system is reduced, small molecules are slowly precipitated to the surface of the adhesive layer, the wettability is increased, and the adhesion is increased.
[0196] Comparative Example 6 uses 3-(4-methoxybenzoyl) acrylic acid as the unsaturated acid. However, due to the steric hindrance of the benzene ring, the double bond addition reaction is hindered, the reaction rate of the acid is low, and there are free acid monomers to produce residual glue. The gel fraction is as low as 80%. The 180° peeling force at room temperature over a year increases significantly, from 261gf / 25mm to 620gf / 25mm, increasing the risk of rework.
[0197] In Comparative Example 7, the acrylic acid content is increased to 12 parts by weight, which is higher than the limit range of the present invention, so that the acrylic acid reaction density is increased, and the gel fraction is 90%. Although the presence of a large number of carboxyl groups increases the anchoring force between the adhesive layer and the adherend, the large gel fraction causes the adhesive to lose its viscoelasticity, resulting in low initial peeling force and poor cohesion. In Comparative Example 8, the acrylic acid content is reduced to 4 parts by weight, which is lower than the limit range of the present invention. The carboxyl content is reduced, the anchoring force to the adherend is reduced, the initial peeling force is low, the gel fraction is 80%, and the cohesion is poor.
[0198] In comparative example 9, the content of 2-hydroxyethyl acrylate is increased to 21 parts by weight, which is higher than the limit range of the present invention, so that the reaction density of 2-hydroxyethyl acrylate is increased, and the gel fraction is 89%. Although the presence of a large amount of hydroxyl groups increases the anchoring force between the adhesive layer and the adherend, the increase in gel fraction causes the adhesive to lose viscoelasticity, resulting in low initial peeling force and poor cohesion. In comparative example 10, the content of 2-hydroxyethyl acrylate is reduced to 9 parts by weight, which is lower than the limit range of the present invention, resulting in a reduction in the raw materials participating in the subsequent post-curing reaction with the isocyanate compound, insufficient post-curing, and inability to fully restrict the migration of low molecular weight free monomers and low polymerization degree molecules. Therefore, the 180° peeling force at room temperature over a year increases significantly, from the initial 218gf / 25mm to 628gf / 25mm.
[0199] In comparative example 11, the content of the crosslinking agent hexamethylene diisocyanate was increased to 11 parts by weight, which was higher than the limit range of the present invention. The excess isocyanate in the post-curing reaction would slowly migrate to the surface of the adhesive layer after one year of storage, and the peeling force would have residual adhesive. In comparative example 12, the content of hexamethylene diisocyanate was reduced to 4 parts by weight, which was lower than the limit range of the present invention. The effect of inhibiting the growth of adhesion during storage at room temperature was poor, and the peeling force at 180° at room temperature after one year increased significantly to 610 gf / 25 mm.
[0200] In comparative example 13, the content of UF-C051 is increased to 72 parts by weight, which is higher than the limit range of the present invention. The amount of main glue is too large, resulting in increased viscosity of the gel and poor application. Due to the low crosslinking density, the edge of the weather resistance test is warped, and the 180° peeling force at room temperature for 1 year increases greatly to 608gf / 25mm. In comparative example 14, the content of UF-C051 is reduced to 28 parts by weight, which is lower than the limit range of the present invention. The ratio of monomer to UF-C051 is increased, the crosslinking density is increased, the gel fraction reaches 92%, the initial peeling force is greatly reduced, the cohesion weight is dropped, and the edge of the weather resistance test is warped.
[0201] Comparative Example 15 is within the scope of protection of the claims, and the weight ratio of 2-hydroxyethyl acrylate to hexamethylene diisocyanate is changed to greater than 3:1, and the effect of inhibiting the growth of adhesion during storage at room temperature is poor. Comparative Example 16 is within the scope of protection of the claims, and the amount of the cross-linking agent hexamethylene diisocyanate is increased to 10 parts by weight, and the molar ratio of the hydroxyl functional group in 2-hydroxyethyl acrylate (M116.08) to the molar ratio of the isocyanate functional group in hexamethylene diisocyanate (M168.19) is 0.724:1. The hexamethylene diisocyanate is excessive, and after one year of storage, the isocyanate compound will slowly migrate to the surface of the adhesive layer, resulting in residual adhesive in the peeling force.
[0202] It should be emphasized that the above are only preferred embodiments of the present invention and do not limit the present invention in any form. Any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A pressure-sensitive adhesive with excellent weather resistance, Features The composition comprises the following components in parts by weight: 。 2. A pressure-sensitive adhesive having excellent weather resistance according to claim 1, Features: The weight ratio of the hydroxyl UV monomer to the crosslinking agent is 1:1 to 3:1, and the molar number of the hydroxyl functional group in the hydroxyl UV monomer is in excess of the molar number of the isocyanate functional group in the crosslinking agent.
3. A pressure-sensitive adhesive having excellent weather resistance according to any one of claims 1 or 2, Features: The weight average molecular weight of the acrylic polyurethane prepolymer is 10,000 to 80,000; the UV hard monomer is a multifunctional acrylate or a multifunctional methacrylate; the photoinitiator is a free radical photoinitiator; the crosslinking agent is an isocyanate compound; the coupling agent is a silane coupling agent; and the antistatic agent is an ionic liquid antistatic agent.
4. A pressure-sensitive adhesive having excellent weather resistance according to claim 3, Features: The acrylic polyurethane prepolymer is selected from UF-C051 of Kyoeisha Co., Ltd., UA-1138P of Shin-Nakamura Co., Ltd., DR-U299 of Changxing Materials Co., Ltd., DR-U282 (molecular weight 20000-30000) of Changxing Materials Co., Ltd., CN9178NS and CN9014NS of Sartomer Co.; The UV hard monomer is any one or more of diacrylate, dimethacrylate, triacrylate, and trimethacrylate; The UV soft monomer is any one or more of tetrahydrofuran acrylate, isooctyl acrylate, butyl acrylate, and ethyl acrylate; The unsaturated acid is any one or more of acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, 4-(3-(acryloyloxy)propoxy)benzoic acid, and crotonic acid; The hydroxyl UV monomer is selected from any one or more of 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl acrylate, 2-hydroxypropyl methacrylate, 4-hydroxybutyl acrylate, 4-hydroxybutyl methacrylate, 6-hydroxyhexyl acrylate, 6-hydroxyhexyl methacrylate, 8-hydroxyoctyl acrylate, 8-hydroxyoctyl methacrylate, 8-hydroxyoctyl acrylate, 8-hydroxyoctyl methacrylate, 6-hydroxyhexyl acrylate, 6-hydroxyhexyl methacrylate, 2-hydroxyethylene glycol acrylate, 2-hydroxyethylene glycol methacrylate, 2-hydroxypropylene glycol acrylate, and 2-hydroxypropylene glycol methacrylate; The photoinitiator is any one or more of 184 photoinitiator, 907 photoinitiator, 1173 photoinitiator, benzophenone, 127 photoinitiator and 2959 photoinitiator; The cross-linking agent is any one or more of butylene diisocyanate, hexamethylene diisocyanate, cyclopentylene diisocyanate, tetramethylene diisocyanate, isophorone diisocyanate, and tetramethylxylylene diisocyanate; The coupling agent is any one of KH550, KH560, KH570, A151, A171 and A172; The antistatic agent is FC4400 from 3M.
5. A pressure-sensitive adhesive having excellent weather resistance according to claim 1, Features: The gel fraction of the pressure-sensitive adhesive after UV curing is 82% to 88%, the initial peeling force on the glass is 200 to 500 gf / 25 mm, and after one year at room temperature, the peeling force on the glass is 300 to 600 gf / 25 mm.
6. A method for preparing a pressure-sensitive adhesive having excellent weather resistance according to any one of claims 1 to 5, Features The following steps are involved: S1. Mix UV hard monomer, UV soft monomer, unsaturated acid, and hydroxyl UV monomer evenly, add coupling agent, antistatic agent, and crosslinking agent, and stir evenly; then add photoinitiator, and stir until dissolved evenly to obtain a mixed solution a; S2. Add the mixed solution a into the acrylic polyurethane prepolymer, stir and mix evenly, and obtain the pressure-sensitive adhesive solution after defoaming, which can be directly used for coating.
7. The method for preparing a pressure-sensitive adhesive having excellent weather resistance according to claim 6, Features: The preparation process and storage environment of the pressure-sensitive adhesive must be protected from light; the prepared adhesive solution must be used within 48 hours.
8. A polarizing film, Features: It comprises a PVA layer (1), an outer protective layer (3) and an inner protective layer (4) adhered to the upper and lower surfaces of the PVA layer (1) via UV adhesive (2), a release film (7) adhered to the outer side of the inner protective layer (4) via a pressure-sensitive adhesive layer (6), and a protective film (5) is arranged on the outer side of the outer protective layer (3); the pressure-sensitive adhesive layer is the pressure-sensitive adhesive according to any one of claims 1 to 5.
9. The polarizer according to claim 8, Features: The thickness of the pressure-sensitive adhesive layer (6) is 10 to 30 μm, and the surface resistance is 9.9×10 11 Ω / □ or less.
10. The polarizer according to claim 8, Features: The UV curing lamp source used for curing the pressure-sensitive adhesive layer (6) is a high-pressure mercury lamp or a halogen lamp, and the UVA curing energy is 1000 mj / cm 2 Above, the light intensity of UVA is 300mw / cm 2 above.
Citation Information
Patent Citations
Polaroid containing UV curing PSA glue and preparation method thereof
CN118707645A
Cited By
High-impact-resistance coating for ultra-thin glass, preparation method and component layer
CN119391290A
A solvent-free UV curing pressure-sensitive adhesive and preparation method thereof
CN119736060A