Aluminum-doped binary inorganic salt fused salt heat storage material with high heat storage density and preparation method of aluminum-doped binary inorganic salt fused salt heat storage material

By doping metal aluminum in high-temperature liquid phase fusion method in binary inorganic salts, the problem of insufficient specific heat capacity and heat storage density of existing binary high-temperature molten salt heat storage materials is solved, and the phase change temperature is achieved without changing The heat storage density is improved, providing higher specific heat capacity and heat diffusion coefficient, and improving heat storage performance.

CN119060693APending Publication Date: 2024-12-03NANJING JINHE ENERGY MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028795.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing binary high-temperature molten salt heat storage materials have lower specific heat capacity and heat storage density. How to improve their energy storage density without changing the phase change temperature.

Method used

Using aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material, the metal aluminum is uniformly doped into binary inorganic chloride salt through high-temperature liquid phase fusion method to prepare a higher specific heat capacity and heat storage density material. The method includes heating the binary inorganic chloride salt in an atmosphere furnace and melting the metal aluminum completely, ensuring uniform dispersion of the aluminum, preventing oxidation, and curing after natural cooling.

Benefits of technology

Without changing the phase transition temperature, the heat storage density of the material is improved by more than 14%, and the composite material is stable after aluminum doping. The phase transition temperature of metal aluminum is consistent with the binary inorganic salt, providing higher specific heat capacity and heat The diffusion coefficient improves the heat storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060693A_ABST
    Figure CN119060693A_ABST
Patent Text Reader

Abstract

The invention discloses an aluminum-doped binary inorganic salt fused salt heat storage material with high heat storage density, and belongs to the technical field of heat storage. Comprising binary inorganic chlorine salt and liquid-phase aluminum, and the content of the liquid-phase aluminum does not exceed 0.9% of the total mass of the heat storage material. The aluminum-doped binary inorganic salt high-heat-storage-density fused salt heat storage material is obtained through a high-temperature liquid phase co-melting method, compared with original binary inorganic salt fused salt, the heat storage density of the material is improved by 14% or above on the premise that the phase change temperature of the material is not changed, the comprehensive heat storage density in the temperature range of 150-700 DEG C exceeds 1043.2 KJ / kg, and the heat storage density of the aluminum-doped binary inorganic salt high-heat-storage-density fused salt heat storage material is improved by 14% or above on the premise that the phase change temperature of the material is not changed. The doped material metal aluminum is uniformly dispersed in the binary inorganic salt, and the composite material is stable, not prone to layering and capable of being used for a long time. The invention also discloses a preparation method of the aluminum-doped binary inorganic salt fused salt heat storage material with high heat storage density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a molten salt heat storage material, in particular to an aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material and a preparation method thereof, belonging to the technical field of heat storage. Background Art

[0002] With the development and progress of science and technology, energy issues have become a hot research hotspot at home and abroad. Using energy storage technology to effectively improve energy utilization and reduce energy waste has become an important technical direction for countries around the world to improve their energy structure. As an important branch of energy storage technology, heat storage technology has the advantages of larger energy storage capacity, lower unit energy storage cost, and wide application compared to other energy storage technologies. The raw materials of sodium chloride-potassium chloride binary inorganic molten salt are easy to obtain, the material is highly safe and low in cost, and it has a suitable phase change temperature, high specific heat capacity and phase change latent heat. It is a commonly used binary high-temperature molten salt heat storage material. However, the existing binary high-temperature molten salt heat storage materials generally have shortcomings such as relatively low specific heat capacity and heat storage density. How to further improve the energy storage density of sodium chloride-potassium chloride binary inorganic molten salt without changing the phase change temperature of the binary inorganic salt is an important research direction in the future. Summary of the invention

[0003] The technical problem to be solved by the present invention is to overcome the defects of the prior art and provide an aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material and a preparation method thereof which can have higher specific heat capacity and heat storage density without changing the phase change temperature of the heat storage material.

[0004] In order to solve the above technical problems, the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material provided by the present invention includes a binary inorganic chloride salt and liquid aluminum, and the content of the liquid aluminum does not exceed 0.9% of the total mass of the heat storage material.

[0005] In the present invention, the binary inorganic salt is a binary chloride molten salt composed of sodium chloride and potassium chloride with a phase transition temperature of 660°C.

[0006] The method for preparing the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material comprises the following steps:

[0007] S1: placing a solid binary inorganic chloride salt at room temperature in a container, fixing it in an atmosphere furnace, and suspending metal aluminum above the container;

[0008] S2: After closing the atmosphere furnace, nitrogen is introduced into the atmosphere furnace, and the air inside the atmosphere furnace is exhausted until the oxygen content is reduced to below 0.1%;

[0009] S3: Start the atmosphere furnace, rotate the container and heat the atmosphere furnace so that the binary inorganic chloride salt undergoes a complete phase change and the metal aluminum is completely melted and evenly doped in the liquid binary inorganic chloride salt; during the heating process, the atmosphere furnace is filled with a protective gas to prevent oxidation of the metal aluminum;

[0010] S4: Naturally cool to room temperature and solidify to obtain aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material.

[0011] In the present invention, the rotation speed of the container in S3 is 30-60RPM, and the heating temperature of the atmosphere furnace is 750-900°C.

[0012] In the present invention, the distance between the metal aluminum and the top of the container is 10 mm.

[0013] In the present invention, the metal aluminum is industrial pure aluminum with a content exceeding 99.5%.

[0014] In the present invention, the protective gas is nitrogen.

[0015] The beneficial effects of the present invention are as follows: (1) an aluminum-doped binary inorganic salt molten salt with high heat storage density is obtained by a high-temperature liquid phase eutectic method. Compared with the original binary inorganic salt molten salt, the heat storage density of the material is increased by more than 14% without changing the phase change temperature of the material. The comprehensive heat storage density exceeds 1043.2 KJ / kg in the temperature range of 150-700°C. The doped material metal aluminum is uniformly dispersed in the binary inorganic salt. The composite material is stable and not prone to stratification and can be used for a long time. (2) The present invention provides a high-temperature liquid phase eutectic method, which solves the problem of poor compatibility between metal materials and inorganic salts. Liquid metal aluminum is uniformly doped in binary inorganic chloride salt at high temperature to construct a Stable composite material structure; the phase transition temperatures of metallic aluminum and binary inorganic chloride salt are consistent, both of which are 660°C. At the same time, the solubility of metallic aluminum in liquid binary inorganic chloride salt is very low, so the phase transition temperature of the binary inorganic salt is not changed after doping; metallic aluminum has a higher specific heat capacity than inorganic chloride salt. At the same time, metallic aluminum doped in binary inorganic salt provides more microscopic heat conduction pathways, improves the thermal diffusion coefficient, and further improves the specific heat capacity and comprehensive heat storage density of the molten salt material; (3) The present invention effectively improves the specific heat capacity and heat storage density of the binary inorganic salt, while not changing the phase transition temperature and application scenario range of the binary inorganic salt, thereby greatly improving the heat storage performance of the binary inorganic salt heat storage material. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0017] Figure 1Schematic diagram of the preparation method of aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material in an embodiment of the present invention;

[0018] Figure 2 A comparison chart of the specific heat capacity of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 1 and the traditional binary inorganic salt;

[0019] Figure 3 A comparison chart of the specific heat capacity of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 2 and the traditional binary inorganic salt;

[0020] Figure 4 A comparison chart of the specific heat capacity of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 3 and the traditional binary inorganic salt;

[0021] Figure 5 A comparison chart of phase change temperature and phase change latent heat of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 1 and the traditional binary inorganic salt;

[0022] Figure 6 A comparison diagram of the phase change temperature and phase change latent heat of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 2 and the traditional binary inorganic salt;

[0023] Figure 7 A comparison chart of the phase change temperature and phase change latent heat of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 3 and the traditional binary inorganic salt;

[0024] Figure 8 This is a comparison diagram of the phase change temperature deviation of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 1 and the traditional binary inorganic salt under the cyclic use state;

[0025] Fig. 9 A comparison diagram of the phase change latent heat attenuation of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in Example 1 and the traditional binary inorganic salt under cyclic use;

[0026] Attached Figure 1 Middle: 1-binary inorganic salt, 2-corundum crucible, 3-silicon nitride turntable, 4-metal aluminum sheet, 5-fixing clamp, 6-high temperature atmosphere furnace, 7-ventilation pipeline. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0028] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Some embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0030] In the preparation process of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material of Example 1, Figure 1 As shown:

[0031] Step 1: 55 g potassium chloride and 44.1 g sodium chloride are uniformly mixed to form a binary inorganic molten salt 1 and then placed in a corundum crucible 2;

[0032] Step 2: Transfer the binary inorganic molten salt 1 and the corundum crucible 2 as a whole and fix them on the silicon nitride turntable 3 in the high-temperature atmosphere furnace 6;

[0033] Step 3: Accurately weigh 0.9 g of a metal aluminum sheet 4, and use a bracket and a fixing clamp 5 to fix the metal aluminum sheet 10 mm above the edge of the corundum crucible to prevent splashing when the molten liquid aluminum falls;

[0034] Step 4: Close the high-temperature atmosphere furnace 6, open the ventilation pipe 7 to introduce nitrogen into it and exhaust the internal air until the oxygen content drops below 0.1%;

[0035] Step 5: Set the speed of the silicon nitride turntable to 48 RPM, set the heating temperature to 820°C, set the heating time to 4 hours, and start the high-temperature atmosphere furnace 6 to start heating. During the heating process, the high-temperature atmosphere furnace is filled with nitrogen to prevent oxidation of the metal aluminum.

[0036] Step 6: After the set time is reached, the heating function of the high-temperature atmosphere furnace 6 is turned off, and the material in the corundum crucible 2 is naturally cooled to room temperature for 24 hours and solidified to obtain 100g of aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material.

[0037] The performance of the phase change material obtained in Example 1 was tested by using a differential scanning calorimeter and a continuous reference method with sapphire as a reference.

[0038] like Figure 2 As shown, the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material obtained in Example 1 has an average specific heat capacity of 1.372 kJ / (kg·K) in the range of 150 to 630° C., which is 16% higher than that of traditional binary inorganic salts.

[0039] like Figure 5 As shown, the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material obtained in Example 1 has almost no change in phase change temperature and phase change latent heat compared to the original binary inorganic salt heat storage material.

[0040] After testing, the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material obtained in Example 1 has stable performance during repeated use, and the phase transition temperature hardly deviates (such as Figure 8 As shown), the latent heat of phase change hardly decays (as shown Fig. 9 shown).

[0041] In the preparation process of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material of Example 2, as Figure 1 As shown:

[0042] Step 1: 55 g potassium chloride and 44.1 g sodium chloride are uniformly mixed to form a binary inorganic molten salt 1 and then placed in a corundum crucible 2;

[0043] Step 2: Transfer the binary inorganic molten salt 1 and the corundum crucible 2 as a whole and fix them on the silicon nitride turntable 3 in the high-temperature atmosphere furnace 6;

[0044] Step 3: Accurately weigh 0.6 g of a metal aluminum sheet 4, and use a bracket and a fixing clamp 5 to fix the metal aluminum sheet 10 mm above the edge of the corundum crucible to prevent splashing when the molten liquid aluminum falls;

[0045] Step 4: Close the high-temperature atmosphere furnace 6, open the ventilation pipe 7 to introduce nitrogen into it and exhaust the internal air until the oxygen content drops below 0.1%;

[0046] Step 5: Set the speed of the silicon nitride turntable to 30 RPM, set the heating temperature to 750°C, set the heating time to 4 hours, and start the high-temperature atmosphere furnace 6 to start heating. During the heating process, the high-temperature atmosphere furnace is filled with nitrogen to prevent oxidation of the metal aluminum.

[0047] Step 6: After the set time is reached, the heating function of the high-temperature atmosphere furnace 6 is turned off, and the material in the corundum crucible 2 is naturally cooled to room temperature for 24 hours and solidified to obtain 99.7g of aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material.

[0048] The performance of the phase change material obtained in Example 2 was tested by using a differential scanning calorimeter and a continuous reference method with sapphire as a reference.

[0049] like Figure 3 As shown in the figure, the average specific heat capacity of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material obtained in Example 2 is 1.266 kJ / (kg·K) in the range of 150 to 630°C, which is 7.1% higher than that of the traditional binary inorganic salt (e.g. Figure 3 ).

[0050] like Figure 6 As shown, the phase change temperature and phase change latent heat of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material obtained in Example 2 are almost unchanged compared to the original binary inorganic salt heat storage material.

[0051] In the preparation process of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material of Example 3, as Figure 1 As shown:

[0052] Step 1: 55 g potassium chloride and 44.1 g sodium chloride are uniformly mixed to form a binary inorganic molten salt 1 and then placed in a corundum crucible 2;

[0053] Step 2: Transfer the binary inorganic molten salt 1 and the corundum crucible 2 as a whole and fix them on the silicon nitride turntable 3 in the high-temperature atmosphere furnace 6;

[0054] Step 3: Accurately weigh 3 g of a metal aluminum sheet 4, and use a bracket and a fixing clamp 5 to fix the metal aluminum sheet 10 mm above the edge of the corundum crucible to prevent splashing when the molten liquid aluminum falls;

[0055] Step 4: Close the high-temperature atmosphere furnace 6, open the ventilation pipe 7 to introduce nitrogen into it and exhaust the internal air until the oxygen content drops below 0.1%;

[0056] Step 5: Set the speed of the silicon nitride turntable to 60RPM, set the heating temperature to 890°C, set the heating time to 8h, and start the high-temperature atmosphere furnace 6 to start heating. During the heating process, the high-temperature atmosphere furnace is filled with nitrogen to prevent oxidation of the metal aluminum.

[0057] Step 6: After the set time is reached, the heating function of the high-temperature atmosphere furnace 6 is turned off, and the material in the corundum crucible 2 is naturally cooled to room temperature for 24 hours and solidified to obtain 102.1g of aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material.

[0058] The performance of the phase change material obtained in Example 3 was tested by using a differential scanning calorimeter and a continuous reference method with sapphire as a reference.

[0059] like Figure 4As shown, the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material obtained in Example 3 has an average specific heat capacity of 1.278 kJ / (kg·K) in the range of 150 to 630° C., which is 8.1% higher than that of traditional binary inorganic salts.

[0060] like Figure 7 As shown, the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material obtained in Example 3 has almost no change in phase change temperature and phase change latent heat compared to the original binary inorganic salt heat storage material, but from a macroscopic perspective, it can be found that aggregated metal particles are irregularly present in the material.

[0061] In the above embodiments 1 to 3, the phase transition temperature of the binary inorganic molten salt 1 composed of sodium chloride and potassium chloride is 660° C. The binary inorganic molten salt 1 in the above embodiments is a relatively common chloride salt, and the fixed ratio of sodium chloride to potassium chloride is also the low eutectic point of the binary system.

[0062] In the above-mentioned embodiments 1 to 3, the metal aluminum sheet 4 is industrial pure aluminum with an aluminum content exceeding 99.5%. Studies have confirmed that the content of liquid aluminum does not exceed 0.9% of the total mass of the obtained heat storage material. When it exceeds 0.9%, the metal aluminum cannot be dissolved in the molten salt in the liquid phase, and will not continue to enhance the heat storage capacity (specific heat capacity) of the material, but will instead reduce the material life.

[0063] Comparison table of relevant parameters of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in each embodiment and the traditional binary chloride salt

[0064]

[0065] It can be seen from the above table that the average specific heat capacity and heat storage density of the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material prepared in each embodiment are significantly better than those of the traditional binary chloride salt, but the phase change temperature, phase change latent heat and service life remain basically the same.

[0066] The present invention provides an aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material and a method for preparing the same. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented using existing technologies.

Claims

1. Aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material, characterized by: It comprises binary inorganic chloride salt and liquid aluminum, wherein the content of the liquid aluminum does not exceed 0.9% of the total mass of the heat storage material.

2. The aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material according to claim 1, characterized in that: The binary inorganic salt is a binary chloride molten salt composed of sodium chloride and potassium chloride with a phase transition temperature of 660°C.

3. The method for preparing the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material according to claim 1 or 2, characterized in that: The steps include: S1: placing a solid binary inorganic chloride salt at room temperature in a container, fixing it in an atmosphere furnace, and suspending metal aluminum above the container; S2: After closing the atmosphere furnace, nitrogen is introduced into the atmosphere furnace, and the air inside the atmosphere furnace is exhausted until the oxygen content is reduced to below 0.1%; S3: Start the atmosphere furnace, rotate the container and heat the atmosphere furnace so that the binary inorganic chloride salt undergoes a complete phase change and the metal aluminum is completely melted and evenly doped in the liquid binary inorganic chloride salt; during the heating process, the atmosphere furnace is filled with a protective gas to prevent oxidation of the metal aluminum; S4: Naturally cool to room temperature and solidify to obtain aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material.

4. The method for preparing the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material according to claim 3, characterized in that: In S3, the rotation speed of the container is 30-60RPM, and the heating temperature of the atmosphere furnace is 750-900°C.

5. The method for preparing the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material according to claim 3, characterized in that: The distance between the metal aluminum and the top of the container is 10 mm.

6. The method for preparing the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material according to claim 3, characterized in that: The metal aluminum is industrial pure aluminum with a content exceeding 99.5%.

7. The method for preparing the aluminum-doped binary inorganic salt high heat storage density molten salt heat storage material according to claim 3, characterized in that: The protective gas is nitrogen.