Water shutoff agent and preparation method thereof
By combining pre-crosslinking weak gel with secondary crosslinking polymer, an impact dilute gel baffle water blocking agent with a porous structure is formed, which solves the problem of traditional water blocking agent under high temperature, high pressure and high mineralization conditions. Stability and impact dilution problems achieve high-strength water blocking effect.
Patent Information
- Application Number
- CN202310633745.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-05-31
AI Technical Summary
Traditional gel water blocking agents have problems such as hydrolysis, precipitation, explosion accumulation, and poor impact dilution resistance in the crack-hole carbonate reservoirs of Northwest Oilfield with high temperature, high pressure and high mineralization, making it difficult to form high-strength and tough sealing. The structure is blocked, and the clay ore fails under high mineralization conditions.
The preparation method of combining pre-crosslinked weak gel with secondary crosslinked polymer is used to form an impact dilute gel with a porous structure by mixing components such as water, chelating agent, polymerized monomer, crosslinking agent and initiator. The baffle water blocking agent uses a secondary crosslinking agent to form an interpenetrating crosslinking network at high temperatures to improve the strength and stability of the water blocking agent.
It has achieved excellent water-resistance and water-blocking ability of the water-blocking agent, and has certain gel time control capabilities to form high-strength baffle gel, effectively avoiding the "pancake spread" phenomenon and improving the body shape of the three-dimensional space The blocking ability of the hole.
Smart Images

Figure CN119060701A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of oilfield profile control and water plugging, and in particular to a water plugging agent and a preparation method thereof. Background Art
[0002] The fracture-cave carbonate reservoirs in Northwest Oilfield have significant geological characteristics such as high temperature, high pressure, and high mineralization. In addition, the geological sedimentary structure, spatial distribution of reservoirs, and internal scale changes of multi-porous medium reservoirs are different from those of conventional single-porous medium sandstone reservoirs. The water plugging of oil wells is different from the water well profile adjustment in terms of pressure gradient distribution, oil-water selectivity, and targeted placement of plugging agents. For fracture-cave carbonate reservoirs with large fractures and cave reservoirs as a whole, water plugging has been widely studied as a relatively effective leading measure for reducing water and increasing oil. The geology of this type of reservoir has the following characteristics: deep burial depth (5000-8000m), high temperature (120-150℃), high mineralization (200,000-220,000 mg / L), and high pressure (50-70MPa); cave-fracture combination, complex and variable scale, and diverse forms of connectivity; strong water energy, prominent contradictions in the horizontal profile, and significant differences in oil and water distribution.
[0003] Faced with high-temperature deep wells and the formation water quality of fracture-cavity carbonate reservoirs in Northwest Oilfield, which is a calcium chloride water type environment, the traditional gel water plugging system has the following technical defects: (1) When the polymer molecular chain is exposed to a high-content metal ion environment, the side groups such as amide and carboxyl groups are easily attacked by divalent calcium and magnesium ions and hydrolyzed and precipitated, which easily leads to the "pancake" phenomenon, making it difficult to form a high-strength and tough plugging structure in the three-dimensional space fracture-cavity position, and it is difficult to form effective retention, and the long-term stability is reduced; (2) High temperature accelerates the polymerization reaction rate of propionic acid condensate monomers, which are easy to explode and gel during the pumping process, and abnormal gelation blocks the wellbore; (3) The traditional gel system is affected by high temperature, resulting in too low viscosity before gelation, and the front position is not resistant to water scouring, and the ability to resist dilution is poor, resulting in delayed gelation time and reduced plugging strength, which is not conducive to the formation of a high-retention and strong and stable baffle gel system; (4) The high mineralization geological characteristics of fracture-cavity carbonate reservoirs in Northwest Oilfield inhibit the dispersion of clay metal cations in water solvents. As the electrolyte concentration in the aqueous solution increases, the hydration of metal ions competes with the hydration of clay for water molecules, reducing the ability of clay to directly adsorb water molecules. Secondly, the number of cations increases, squeezing the diffusion layer, resulting in the thinning of the clay hydration film and weakening of the hydration capacity. Therefore, under the special high-mineralization geological conditions of the Northwest oil reservoirs, the method of using clay minerals to increase the liquid phase viscosity of the water body to achieve anti-thinning is not feasible. Summary of the invention
[0004] One of the present inventions provides a method for preparing a water plugging agent, which comprises the following steps:
[0005] 1) mixing water, a first chelating agent, a polymerization monomer, a primary cross-linking agent, an initiator and an accelerator to obtain a liquid A;
[0006] 2) mixing water, the second chelating agent, the cross-linked polymer, the secondary cross-linking agent and the stabilizer to obtain liquid B;
[0007] 3) Liquid A and liquid B are mixed evenly to obtain the water plugging agent.
[0008] In one embodiment, the first chelating agent and the second chelating agent are independently sodium carbonate.
[0009] In a specific embodiment, the polymerizable monomers are amide monomers, sulfonate monomers and hydrophobic associating monomers.
[0010] In a specific embodiment, the amide monomer is acrylamide and / or N,N-dimethylacrylamide.
[0011] In a specific embodiment, the sulfonate monomer is at least one of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, sodium styrene sulfonate and sodium allyl sulfonate.
[0012] In a specific embodiment, the hydrophobic associating monomer is at least one of octadecyltrimethylammonium chloride and / or hexadecyltrimethylammonium bromide.
[0013] In a specific embodiment, based on the mass of the polymerized monomer as 100%, the content of the acrylamide monomer is 60% to 78%, the content of the sulfonate monomer is 20% to 35%, and the content of the hydrophobic associating monomer is 2% to 5%.
[0014] In a specific embodiment, the primary cross-linking agent is N,N-methylenebisacrylamide.
[0015] In a specific embodiment, the secondary crosslinking agent is at least one of hexamethylenetetramine, resorcinol, p-phenylenediamine, zirconium acetate and chromium acetate.
[0016] In a specific embodiment, the initiator is dicumyl peroxide and / or tert-butyl hydroperoxide.
[0017] In a specific embodiment, the accelerator is tetramethylethylenediamine.
[0018] In a specific embodiment, the cross-linked polymer is at least one of partially hydrolyzed polyacrylamide, partially hydrolyzed polyacrylonitrile and acrylamide-acrylic acid-octadecyltrimethylammonium chloride copolymer.
[0019] In a specific embodiment, the viscosity average molecular weight of the partially hydrolyzed polyacrylamide is 15 million to 18 million, and the degree of hydrolysis is 20% to 25%.
[0020] In a specific embodiment, the viscosity average molecular weight of the partially hydrolyzed polyacrylonitrile is 15 million to 18 million, and the degree of hydrolysis is 35% to 40%.
[0021] In a specific embodiment, the viscosity average molecular weight of the acrylamide-acrylic acid-octadecyltrimethylammonium chloride copolymer is 15 million to 18 million.
[0022] In one embodiment, the stabilizer is thiourea.
[0023] In a specific embodiment, based on the mass of the liquid A being 100%, the content of the first chelating agent is 2% to 4%, and the content of the polymerizable monomer is 3% to 6%.
[0024] In a specific embodiment, based on the mass of the polymerized monomer as 100%, the content of the primary crosslinking agent is 1% to 5%; the content of the accelerator is 0.1% to 0.2%; and the content of the initiator is 0.5% to 1%.
[0025] In a specific embodiment, based on the mass of the B liquid as 100%, the content of the second chelating agent is 3% to 6%, the content of the cross-linked polymer is 0.4% to 1.2%, the content of the secondary cross-linking agent is 0.5% to 1.5%; and the content of the stabilizer is 0.05% to 0.1%.
[0026] The second invention provides the water plugging agent prepared by the preparation method described in any one of the first inventions.
[0027] Beneficial effects of the present invention:
[0028] (1) Excellent resistance to water dilution. Conventional polymer gel-type water plugging agents mainly include polymer cross-linking systems and monomer polymerization systems. Water-soluble polymers or monomers are often used as reaction reagents. After contacting with formation water in a high-temperature environment, they are dispersed and diluted, and the gel quality deteriorates or even becomes difficult to gel. The present invention uses pre-cross-linked weak gel as the primary structure, and the injected water is mechanically encapsulated in the pores of the gel with a porous structure, thereby improving the ability to resist formation water dilution.
[0029] (2) Excellent water plugging ability. Secondary water-soluble crosslinking agents such as hexamethylenetetramine are hidden inside the pre-crosslinked weak gel. As the ambient temperature rises, the reactive substances or catalysts are released, and the aldehyde groups or aromatic amine groups react with the amide groups in the primary structure to form a secondary interpenetrating crosslinking network, which further improves the strength of the water plugging agent and plays the role of a front baffle.
[0030] (3) It has a certain ability to regulate gel time. The amide group hydrolyzes at high temperature to form a carboxylic acid group, which reduces the reaction activity and causes the gel strength to decrease. The cyano group in partially hydrolyzed polyacrylonitrile can be hydrolyzed into an amide group. At the same time, the hexamethylenetetramine crosslinker hydrolyzes with increasing temperature to generate a reactive aldehyde group, thereby reserving more potential reactive sites and improving the ability to regulate gel time in a high temperature environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The state diagram of the water plugging agent prepared in Example 1 after curing for 5 hours at natural ambient temperature is shown.
[0032] Figure 2 The state diagram of the water plugging agent prepared in Example 1 when placed at 140°C for 5 hours is shown.
[0033] Figure 3 The state diagram of the water plugging agent prepared in Comparative Example 1 when placed at 140°C for 5 hours is shown.
[0034] Figure 4 The state diagram of the water plugging agent prepared in Comparative Example 2 when placed at 140°C for 5 hours is shown.
[0035] Figure 5 The scanning electron microscope observation image of the water plugging agent prepared in Example 1 after curing for 5 hours at natural ambient temperature is shown.
[0036] Figure 6 The scanning electron microscope observation image of the water plugging agent prepared in Example 1 placed at 140° C. for 5 hours is shown. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with examples, but the examples of the present invention are only exemplary descriptions, and the implementation methods do not constitute limitations of the present invention under any circumstances.
[0038] The contents of various mineral ions in the formation water used in the following examples are shown in Table 1.
[0039] Table 1 Concentrations of various mineral ions in the formation water used in various embodiments of the present invention
[0040]
[0041] Example 1
[0042] A method for preparing an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure, comprising the following steps:
[0043] (1) 3 g of chelating agent sodium carbonate, 4.5 g of polymerizable monomer, 135 mg (3% of the total weight of the monomer) of primary crosslinking agent N,N-methylenebisacrylamide, 6.75 mg of accelerator tetramethylethylenediamine (0.15% of the total weight of the monomer), and 33.75 mg of initiator diisopropylbenzene peroxide (0.75% of the total weight of the monomer) were added to 92.5 g of formation water in sequence, and the mixture was stirred evenly to obtain liquid A;
[0044] The total mass of the polymerizable monomers is calculated as 100%, including 3.105 g (mass fraction 69%) of acrylamide, 1.2375 g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate (mass fraction 27.5%) and 0.1575 g of octadecyltrimethylammonium chloride (mass fraction 3.5%);
[0045] (2) 4.5 g of chelating agent sodium carbonate, 0.8 g of partially hydrolyzed polyacrylamide (viscosity average molecular weight 18 million, hydrolysis degree 25%), 1 g of secondary crosslinking agent (a combination of 0.5 g of hexamethylenetetramine and 0.5 g of resorcinol), and 0.075 g of stabilizer thiourea were added to 93.625 g of formation water in sequence and stirred evenly to obtain liquid B;
[0046] (3) Liquid A and liquid B are mixed evenly to obtain an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure.
[0047] Example 2
[0048] A method for preparing an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure, comprising the following steps:
[0049] (1) Add 2 g of chelating agent sodium carbonate, 3 g of polymerizable monomer, 150 mg (5% of the total weight of the monomer) of primary crosslinking agent N,N-methylenebisacrylamide, 3 mg of accelerator tetramethylethylenediamine (0.1% of the total weight of the monomer), and 15 mg of initiator diisopropylbenzene peroxide (0.5% of the total weight of the monomer) to 95 g of formation water, and stir evenly to obtain liquid A;
[0050] Taking the total mass of the polymerized monomers as 100%, the mixture includes 2.25 g acrylamide and 0.09 g N,N-dimethylacrylamide (total mass fraction 78%), 0.6 g sodium 3-allyloxy-2-hydroxy-1-propanesulfonate (mass fraction 20%) and 0.06 g octadecyltrimethylammonium chloride (mass fraction 2%);
[0051] (2) 6 g of chelating agent sodium carbonate, 0.4 g of partially hydrolyzed polyacrylonitrile (viscosity average molecular weight 18 million, hydrolysis degree 40%), 0.5 g of secondary crosslinking agent (a combination of 0.4 g of p-phenylenediamine and 0.1 g of zirconium acetate), and 0.1 g of stabilizer thiourea were added to 93 g of formation water in sequence and stirred evenly to obtain liquid B;
[0052] (3) Liquid A and liquid B are mixed evenly to obtain an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure.
[0053] Example 3
[0054] A method for preparing an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure, comprising the following steps:
[0055] (1) 4 g of chelating agent sodium carbonate, 6 g of polymerizable monomer, 60 mg (1% of the total weight of the monomer) of primary crosslinking agent N,N-methylenebisacrylamide, 12 mg of accelerator tetramethylethylenediamine (0.2% of the total weight of the monomer), and 60 mg of initiator tert-butyl hydroperoxide (1% of the total weight of the monomer) were added to 90 g of formation water in sequence and stirred evenly to obtain liquid A;
[0056] The total mass of the polymerized monomers is taken as 100%, including 3.6 g N,N-dimethylacrylamide (total mass fraction 60%), 2.1 g sodium allyl sulfonate (mass fraction 35%) and 0.3 g hexadecyltrimethylammonium bromide (mass fraction 5%);
[0057] (2) 3 g of chelating agent sodium carbonate, 1.2 g of acrylamide-acrylic acid-octadecyltrimethylammonium chloride copolymer (viscosity average molecular weight 18 million), 1.5 g of secondary crosslinking agent (a composition of 1 g of p-phenylenediamine and 0.5 g of chromium acetate), and 0.075 g of stabilizer thiourea were added to 94.225 g of formation water in sequence and stirred evenly to obtain liquid B;
[0058] (3) Liquid A and liquid B are mixed evenly to obtain an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure.
[0059] Example 4
[0060] A method for preparing an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure, comprising the following steps:
[0061] (1) 3 g of chelating agent sodium carbonate and 5 g of polymerized monomer were added to 92 g of formation water in sequence, and then 150 mg (3% of the total weight of the monomer) of primary crosslinking agent N,N-methylenebisacrylamide, 8.5 mg of accelerator tetramethylethylenediamine (0.17% of the total weight of the monomer), and 37.5 mg of initiator tert-butyl hydroperoxide (0.75% of the total weight of the monomer) were added and stirred evenly to obtain liquid A;
[0062] The total mass of the polymerized monomers is taken as 100%, including 3.5 g acrylamide (total mass fraction 70%), 1.375 g sodium styrene sulfonate (mass fraction 27.5%) and 0.125 g octadecyltrimethylammonium chloride (mass fraction 2.5%);
[0063] (2) 6 g of chelating agent sodium carbonate, 1.2 g of acrylamide-acrylic acid-octadecyltrimethylammonium chloride copolymer (viscosity average molecular weight 15 million), 1.5 g of secondary crosslinking agent (a combination of 0.75 g of hexamethylenetetramine and 0.75 g of resorcinol), and 0.1 g of stabilizer thiourea were added to 91.2 g of formation water in sequence and stirred evenly to obtain liquid B;
[0064] (3) Liquid A and liquid B are mixed evenly to obtain an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure.
[0065] Example 5
[0066] A method for preparing an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure, comprising the following steps:
[0067] (1) 3 g of chelating agent sodium carbonate and 5 g of polymerized monomer were added to 92 g of formation water in sequence, and then 150 mg (3% of the total weight of the monomer) of primary crosslinking agent N,N-methylenebisacrylamide, 8.5 mg of accelerator tetramethylethylenediamine (0.17% of the total weight of the monomer), and 37.5 mg of initiator tert-butyl hydroperoxide (0.75% of the total weight of the monomer) were added and stirred evenly to obtain liquid A;
[0068] The total mass of the polymerized monomers is taken as 100%, including 3.5 g (mass fraction 70%) of acrylamide, 1.4 g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate (mass fraction 28%) and 0.1 g of octadecyltrimethylammonium chloride (mass fraction 2%);
[0069] (2) 3 g of chelating agent sodium carbonate, 0.4 g of partially hydrolyzed polyacrylamide (viscosity average molecular weight 15 million, hydrolysis degree 20%), 0.5 g of secondary crosslinking agent (a combination of 0.25 g of p-phenylenediamine and 0.25 g of zirconium acetate), and 0.05 g of stabilizer thiourea were added to 96.05 g of formation water in sequence and stirred evenly to obtain liquid B;
[0070] (3) Liquid A and liquid B are mixed evenly to obtain an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure.
[0071] Example 6
[0072] A method for preparing an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure, comprising the following steps:
[0073] (1) 4 g of chelating agent sodium carbonate and 3 g of polymerized monomer were added to 93 g of formation water in sequence, and then 30 mg (accounting for 1% of the total weight of the monomer) of primary crosslinking agent N,N-methylenebisacrylamide, 4.5 mg of accelerator tetramethylethylenediamine (accounting for 0.15% of the total weight of the monomer), and 22.5 mg of initiator diisopropylbenzene peroxide (accounting for 0.75% of the total weight of the monomer) were added and stirred evenly to obtain liquid A;
[0074] The total mass of the polymerized monomers is taken as 100%, including 3.5 g (mass fraction 70%) of acrylamide, 1.4 g of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate (mass fraction 28%) and 0.1 g of octadecyltrimethylammonium chloride (mass fraction 2%);
[0075] (2) 6 g of chelating agent sodium carbonate, 0.8 g of partially hydrolyzed polyacrylonitrile (viscosity average molecular weight 15 million, hydrolysis degree 35%), 0.5 g of secondary crosslinking agent (a combination of 0.25 g of p-phenylenediamine and 0.25 g of zirconium acetate), and 0.05 g of stabilizer thiourea were added to 92.65 g of formation water in sequence and stirred evenly to obtain liquid B;
[0076] (3) Liquid A and liquid B are mixed evenly to obtain an impact-resistant dilute gel baffle water plugging agent based on a secondary cross-linking structure.
[0077] Comparative Example 1
[0078] This comparative example provides a method for preparing a water plugging agent, the steps of which are:
[0079] To 98.125 g of formation water, 0.8 g of partially hydrolyzed polyacrylamide (viscosity-average molecular weight 18 million, hydrolysis degree 25%), 1 g of a cross-linking agent (a composition of 0.5 g of hexamethylenetetramine and 0.5 g of resorcinol), and 0.075 g of a stabilizer thiourea were added in sequence and stirred evenly to obtain a water plugging agent.
[0080] Comparative Example 2
[0081] This comparative example provides a method for preparing a water plugging agent, the steps of which are:
[0082] To 93.625 g of formation water, 4.5 g of chelating agent sodium carbonate, 0.8 g of partially hydrolyzed polyacrylamide (viscosity-average molecular weight 18 million, hydrolysis degree 25%), 1 g of cross-linking agent (a composition of 0.5 g of hexamethylenetetramine and 0.5 g of resorcinol), and 0.075 g of stabilizer thiourea were added in sequence and stirred evenly to obtain a water plugging agent.
[0083] Performance evaluation of water plugging agent
[0084] The water plugging agents prepared in Examples 1 to 6 and Comparative Examples 1 and 2 were cured at natural ambient temperature for 5 h, and the apparent gel strength of the water plugging agents was observed by visual code method, and the apparent viscosity was measured by Brookfield viscometer. The results are shown in Table 1. Subsequently, they were placed in a closed metal curing kettle and pressurized to 1.0 MPa with nitrogen (the purpose of pressurization is to ensure that the ambient pressure is higher than the saturated vapor pressure of the solvent at this temperature, thereby avoiding the actual temperature in the container being lower than the design temperature due to solvent evaporation). The closed metal curing kettle was placed in an electric constant temperature blast drying oven and cured at a high temperature of 140°C for 5 h. The closed metal curing kettle was taken out and waited to be restored to the natural ambient temperature. The pressure in the metal curing kettle was released. At this time, the apparent gel strength of the water plugging agent was observed by visual code method, and the elastic modulus was measured by MARSIII Haake rheometer. The results are shown in Table 1. Among them, the visual code method given in the Chinese patent CN 109181664B "A heat-resistant gel plugging agent of phenylenediamine cross-linked polyacrylamide and its preparation method" is used to evaluate the gel strength of the water plugging agent with different curing times.
[0085] Figure 1 This is a diagram of the gelation state of the water plugging agent prepared in Example 1 after curing for 5 hours at natural ambient temperature.
[0086] Figure 2 This is a diagram of the gelation state of the water plugging agent prepared in Example 1 after curing at 140°C for 5 hours.
[0087] Figure 3 This is a diagram of the gelation state of the water plugging agent prepared in Comparative Example 1 after curing at 140°C for 5 hours.
[0088] Figure 4 This is a diagram of the gelation state of the water plugging agent prepared in Comparative Example 2 after curing at 140°C for 5 hours.
[0089] Figure 5 This is the scanning electron microscope observation result of the water plugging agent prepared in Example 1 after curing for 5 hours at natural ambient temperature.
[0090] Figure 6 This is the scanning electron microscope observation result of the water plugging agent prepared in Example 1 after curing at 140°C for 5 hours.
[0091] Table 1
[0092]
[0093] According to the experimental results in Table 1, we can see that:
[0094] (1) After curing for 5 hours at natural ambient temperature, the macroscopic morphology of the primary cross-linked product is a viscous, high-fluidity weak gel, with an apparent viscosity in the range of 1500 mPa·s to 2500 mPa·s, and a strength code of B. Since the prepolymer exists in the form of covalent cross-linking, the water plugging agent is endowed with good resistance to water dilution and water scouring, which is conducive to the stable advancement of the front edge position of the fracture-hole porous medium and avoids the occurrence of the "pancake phenomenon". After high-temperature curing at 140°C for 5 hours, the mechanical strength of the secondary cross-linked product is improved from B grade to G grade or H grade, and the elastic modulus is in the range of 1000Pa to 1600Pa. At the same time, combined with the results of scanning electron microscopy observation, the network structure of the gel product after secondary cross-linking is denser than that of the primary pre-cross-linked weak gel, and the mesh formed by the interlaced chain bundles is also smaller, which further proves the improvement of the mechanical properties of the gel after secondary cross-linking. In this way, through secondary cross-linking, the plugging ability of the three-dimensional space fracture hole is further enhanced, playing the role of the front baffle.
[0095] (2) After curing for 5 hours at natural ambient temperature, the plugging agents prepared in Comparative Examples 1 and 2 have low apparent viscosity. Since the viscosity contribution at this time is mainly provided by linear polymers such as partially hydrolyzed polyacrylamide, the water dilution resistance and flushing ability are weaker than those of the pre-crosslinked weak fluid gels in Examples 1 to 5. After high-temperature curing at 140°C for 5 hours, although the mechanical strength is improved, the strength code can reach Grade D, and the elastic modulus is close to 500Pa, the amide group is easily hydrolyzed to form a carboxylic acid group in a high-temperature and high-salt environment, and the reaction conditions of the carboxylic acid group are difficult to adapt to the temperature and pressure environment of the reservoir, and it has not yet been used as a covalent crosslinking site. Its mechanical properties are still far lower than those of the double network gel formed by the secondary crosslinking in Examples 1 to 5, which is insufficient to effectively plug the three-dimensional fractures and holes.
[0096] Combining and comparing the experimental results of the embodiments and the comparative examples, the following three conclusions can be drawn: (1) The mechanical strength of the primary cross-linked polymer alone is low, and it is difficult to form a high-strength and tough baffle structure; (2) The primary pre-cross-linked fluid weak gel formed by the polymerization of acrylamide monomers exists in the form of covalent cross-linking, which gives the water plugging agent good resistance to water dilution and water erosion; (3) The primary structure formed by the polymerization of acrylamide monomers and the secondary structure formed by the cross-linked polymer are interlaced to form a polymer interpenetrating network system gel, which can improve the gelation performance of a single polymer network.
[0097] Although the present invention has been described with reference to specific embodiments, it will be appreciated by those skilled in the art that various changes may be made without departing from the true spirit and scope of the present invention. In addition, the subject matter, spirit and scope of the present invention may be varied to accommodate specific situations, materials, material combinations and methods. All of these changes are included within the scope of the claims of the present invention.
Claims
1. A method for preparing a water plugging agent, comprising the following steps: 1) mixing water, a first chelating agent, a polymerization monomer, a primary cross-linking agent, an initiator and an accelerator to obtain a liquid A; 2) mixing water, the second chelating agent, the cross-linked polymer, the secondary cross-linking agent and the stabilizer to obtain liquid B; 3) Liquid A and liquid B are mixed evenly to obtain the water plugging agent.
2. The preparation method according to claim 1, It is characterized in that The first chelating agent and the second chelating agent are independently sodium carbonate.
3. The preparation method according to claim 1, It is characterized in that The polymerizable monomers are amide monomers, sulfonate monomers and hydrophobic associating monomers; Preferably, the amide monomer is acrylamide and / or N,N-dimethylacrylamide; Preferably, the sulfonate monomer is at least one of sodium 3-allyloxy-2-hydroxy-1-propanesulfonate, sodium styrenesulfonate and sodium allylsulfonate; Preferably, the hydrophobic associating monomer is at least one of octadecyltrimethylammonium chloride and / or hexadecyltrimethylammonium bromide; Preferably, based on the mass of the polymerized monomer as 100%, the content of the acrylamide monomer is 60% to 78%, the content of the sulfonate monomer is 20% to 35%, and the content of the hydrophobic associating monomer is 2% to 5%.
4. The preparation method according to claim 1, It is characterized in that The primary cross-linking agent is N,N-methylenebisacrylamide; and / or The secondary crosslinking agent is at least one of hexamethylenetetramine, resorcinol, p-phenylenediamine, zirconium acetate and chromium acetate.
5. The preparation method according to claim 1, It is characterized in that The initiator is dicumyl peroxide and / or tert-butyl hydroperoxide.
6. The preparation method according to claim 1, It is characterized in that The accelerator is tetramethylethylenediamine.
7. The preparation method according to claim 1, It is characterized in that The cross-linked polymer is at least one of partially hydrolyzed polyacrylamide, partially hydrolyzed polyacrylonitrile and acrylamide-acrylic acid-octadecyltrimethylammonium chloride copolymer; Preferably, the viscosity-average molecular weight of the partially hydrolyzed polyacrylamide is 15 million to 18 million, and the degree of hydrolysis is 20% to 25%; Preferably, the viscosity-average molecular weight of the partially hydrolyzed polyacrylonitrile is 15 million to 18 million, and the degree of hydrolysis is 35% to 40%; Preferably, the viscosity average molecular weight of the acrylamide-acrylic acid-octadecyltrimethylammonium chloride copolymer is 15 million to 18 million.
8. The preparation method according to claim 1, It is characterized in that The stabilizer is thiourea.
9. The preparation method according to claim 1, It is characterized in that Taking the mass of the liquid A as 100%, the content of the first chelating agent is 2% to 4%, and the content of the polymerizable monomer is 3% to 6%; Preferably, based on the mass of the polymerized monomer as 100%, the content of the primary crosslinking agent is 1% to 5%; the content of the accelerator is 0.1% to 0.2%; and the content of the initiator is 0.5% to 1%; and / or Taking the mass of the B liquid as 100%, the content of the second chelating agent is 3% to 6%, the content of the cross-linked polymer is 0.4% to 1.2%, the content of the secondary cross-linking agent is 0.5% to 1.5%; and the content of the stabilizer is 0.05% to 0.1%.
10. The water plugging agent prepared according to the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
A temperature-resistant gel plugging agent of phenylenediamine crosslinked polyacrylamide and its preparation method
CN109181664B
Chemical secondary-crosslinking jelly foam water plugging and profile controlling liquid
CN102604606A
Secondary crosslinking, profile modification and profile control agent, and preparation method and application thereof
CN103468230A
Hydrophobic associating crosslinked microspheres and preparation method thereof
CN104926987A
Amphoteric crosslinked polymer coil and preparation method thereof
CN106467598A
Cited By
Water shutoff agent for oil field and preparation method of water shutoff agent
CN119931620A