PbS colloidal quantum dot film and preparation method and application thereof

By introducing an alumina dielectric layer into the colloidal quantum dot film, the stability of colloidal quantum dots under high temperature, high electric field and irradiation is solved, and the overall performance and commercial prospects of the device are improved.

CN119060719APending Publication Date: 2024-12-03HUAZHONG UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311787205.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-25
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Colloidal quantum dots are instable under the action of high temperature, high electric field and radiation factors, resulting in a decline in device performance, and it is difficult for the existing technology to effectively improve their stability.

Method used

Colloidal quantum dot coating film with metal halides exchanged as ligands is used to generate two-dimensional perovskite precipitation by dropping the organic halide solution, and an alumina dielectric layer is deposited on the cleaning film to replace the unstable metal halide medium layer to improve the high temperature, electric field and light stability of the device.

Benefits of technology

It significantly improves the stability of PbS colloidal quantum dot film under high temperature, strong electric field and strong light, enhances mobility, and promotes the commercialization of colloidal quantum dot detection technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119060719A_ABST
    Figure CN119060719A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of quantum dots, in particular to a PbS colloidal quantum dot film and a preparation method and application thereof.The preparation method of the PbS colloidal quantum dot film comprises the steps that colloidal quantum dots with metal halide as ligand exchange are taken for film coating, and a colloidal quantum dot precursor film is obtained; dispersing and dissolving organic halide to obtain an organic halide solution; dropwise adding an organic halide solution on the surface of the colloidal quantum dot precursor film and covering the colloidal quantum dot precursor film, after standing, throwing out redundant organic halide solution, and drying to obtain a two-dimensional perovskite precipitation film; cleaning the residual organic halide solution and the two-dimensional perovskite precipitate on the two-dimensional perovskite precipitate film to obtain a cleaned film; and depositing aluminum oxide on the cleaned film to obtain the PbS colloidal quantum dot film. The PbS colloidal quantum dot film has the effect of improving the stability of the PbS colloidal quantum dot film under high temperature, strong electric field and strong light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of quantum dots, and in particular to a PbS colloidal quantum dot film and a preparation method and application thereof. Background Art

[0002] Short-wave infrared detection is widely used in fields such as autonomous driving, medical imaging, and machine vision. The mainstream technology for short-wave infrared detection is photodetectors based on semiconductor materials such as indium gallium arsenide. Currently, indium gallium arsenide photodetectors are extremely expensive due to problems such as high-precision bonding and interconnection and large-size substrate growth. Colloidal quantum dots, as a zero-dimensional semiconductor, have a band gap that matches the short-wave infrared band. Their preparation and processing costs are much lower than traditional indium gallium arsenide semiconductor detectors, so they are an extremely promising short-wave infrared detection technology.

[0003] Halogen elements are often used as ligand molecules in colloidal quantum dots. Liquid-phase ligand exchange based on the phase transfer principle is the most commonly used method, and the prepared colloidal quantum dot infrared detector has a high photoelectric conversion efficiency, which is one of the technical routes with the best performance and the broadest commercial prospects. In order to achieve a good ligand passivation effect, many colloidal quantum dot technologies, including lead sulfide (PbS) quantum dots, use high-concentration halogen-containing salt solutions to complete liquid-phase ligand exchange. For example, the preparation method of large-size lead sulfide colloidal quantum dots, quantum dot films and devices for passivating the (100) surface discloses that large-size (diameter d>4nm) PbS CQDs are bridged to the charge-neutral (100) surface through halide perovskite heteroepitaxial growth.

[0004] Regarding the above-mentioned related technologies, there is a problem that colloidal quantum dots become unstable under the influence of high temperature, high electric field and radiation factors. Summary of the invention

[0005] In order to improve the stability of PbS colloidal quantum dot film under high temperature, high electric field and radiation factors, the purpose of this application is to provide a PbS colloidal quantum dot film and a preparation method and application thereof.

[0006] In the first aspect, the preparation method of the PbS colloidal quantum dot film provided in the present application adopts the following technical scheme:

[0007] A method for preparing a PbS colloidal quantum dot film comprises the following steps:

[0008] Taking a colloidal quantum dot coating film exchanged with a metal halide as a ligand to obtain a colloidal quantum dot precursor film;

[0009] dispersing and dissolving an organic halide to obtain an organic halide solution;

[0010] Add an organic halide solution dropwise onto the surface of the colloidal quantum dot precursor film to cover it, shake off excess organic halide solution after standing, and dry to obtain a two-dimensional perovskite precipitate film;

[0011] cleaning the residual organic halide solution and the two-dimensional perovskite precipitate on the two-dimensional perovskite precipitate film to obtain a cleaned film;

[0012] Aluminum oxide is deposited on the cleaned film to obtain a PbS colloidal quantum dot film.

[0013] By adopting the above technical scheme, a large amount of metal-halogen compounds exist in the colloidal quantum dot precursor film obtained by using metal halide as ligand exchange. Excessive metal-halogen compounds will decompose under the action of light, crystallize under the action of high temperature, and cause ion migration under the action of strong electric field, which seriously restricts the high temperature, electric field and irradiation stability of colloidal quantum dot devices. In the present application, a chemical solution that can react with the metal halide inside the colloidal quantum dot precursor film to generate a two-dimensional perovskite precipitate is added to the surface of the colloidal quantum dot precursor film. The two-dimensional perovskite precipitate can be specifically dissolved without destroying the surface ligands and lattice structure of the original quantum dots. Therefore, the two-dimensional perovskite generated by the reaction is further dissolved by a solution that can specifically dissolve the two-dimensional perovskite precipitate, and finally an inert dielectric layer of aluminum oxide is introduced into the cleaned gap by atomic layer deposition. In summary, the unstable metal halide is reduced, and the mobility and stability can be effectively improved by filling the inert dielectric layer and introducing a dielectric layer with a suitable dielectric constant. Ultimately, the preparation of PbS colloidal quantum dot films with high stability under high temperature, strong electric field, and strong light is achieved, which greatly promotes the commercialization of colloidal quantum dot detection technology and is expected to promote the development and progress of related applications.

[0014] Optionally, the preparation method of the colloidal quantum dot precursor film is:

[0015] Taking colloidal quantum dots with oleic acid as ligand and dissolving them in n-octane to obtain an oleic acid quantum dot solution;

[0016] preparing a metal-halide ligand solution;

[0017] Adding the oleic acid quantum dot solution to the metal-halide ligand solution, stirring and then standing to obtain a metal-halide exchange solution;

[0018] Purifying the metal-halide exchange solution to obtain colloidal quantum dots using metal halides as ligands for exchange;

[0019] The colloidal quantum dots exchanged with metal halide as ligand are dissolved in a spin coating liquid to obtain a slurry, wherein the spin coating liquid is an amine low boiling point solvent;

[0020] The slurry is spin-coated on the surface of the substrate to obtain a colloidal quantum dot precursor film.

[0021] By adopting the above technical scheme, liquid-phase ligand exchange is carried out between metal-halide ligand solution and oleic acid quantum dot solution, halogen is introduced, and the point conversion efficiency of device preparation is improved. The spin coating solvent adopts amine low-boiling point solvent to facilitate spin coating film formation.

[0022] Optionally, the spin coating liquid further comprises a polar organic solvent, and the volume ratio of the polar organic solvent to the amine low boiling point solvent is 1-4:1.

[0023] By adopting the above technical solution, a polar solvent system is introduced into the spin coating liquid to promote the formation of two-dimensional perovskite precipitation, improve the removal efficiency of metal halides, and facilitate the formation of a more uniform aluminum oxide filling distribution in the later stage.

[0024] Optionally, the polar organic solvent is at least one of N,N-dimethylformamide and dimethyl sulfoxide.

[0025] By adopting the above technical solution, N,N-dimethylformamide and dimethyl sulfoxide are both strong polar solvents, which further promote the formation of two-dimensional perovskite precipitation, so that the metal halide is removed more thoroughly and the uniformity of the aluminum oxide filling distribution is improved.

[0026] Optionally, the spin-coating liquid further comprises pyridine derivatives, and the pyridine derivatives account for 0.1-5% of the total volume of the spin-coating liquid.

[0027] By adopting the above technical solution, on the basis of introducing a polar solvent system, pyridine derivatives are further introduced to promote the uniformity of film formation of the solution under the polar system, and further improve the uniformity of subsequent alumina filling distribution.

[0028] Optionally, the residual organic halide solution and the two-dimensional perovskite precipitate on the two-dimensional perovskite precipitate film are cleaned, specifically by repeatedly adding acetonitrile or methanol solution to the surface of the two-dimensional perovskite precipitate film and then drying it.

[0029] By adopting the above technical scheme, the acetonitrile or methanol solution specifically dissolves the two-dimensional perovskite precipitate without destroying the surface ligands and lattice structure of the colloidal quantum dot precursor film, thereby achieving the purpose of cleaning the two-dimensional perovskite precipitate and simultaneously cleaning the residual organic halide solution.

[0030] Optionally, the organic halide is at least one of phenethylammonium iodide, methylamine iodide, p-fluorophenethylammonium iodide, phenethylammonium bromide, and fluoroethylammonium bromide.

[0031] By adopting the above technical scheme, at least one of phenethylammonium iodide, methylamine iodide, p-fluorophenethylammonium iodide, phenethylammonium bromide, and fluoroethylammonium bromide can react with the metal halide inside the colloidal quantum dot precursor film to generate a specifically soluble two-dimensional perovskite precipitate.

[0032] Optionally, the aluminum oxide is deposited on the cleaning film by:

[0033] Trimethylaluminum and water are used as precursor raw materials, and 5 to 30 growth cycles are performed with a pulse time of 0.1 s and a purge time of 10 to 100 s.

[0034] By adopting the above technical solution, a uniformly filled aluminum oxide dielectric layer is formed on the cleaning film.

[0035] In the second aspect, the PbS colloidal quantum dot film provided in this application adopts the following technical solution:

[0036] The PbS colloidal quantum dot film is prepared by using the preparation method of the PbS colloidal quantum dot film.

[0037] By adopting the above technical solution, most of the metal-halide dielectric layer in the colloidal quantum dot precursor film is removed and replaced with a stable aluminum oxide dielectric layer, thereby improving the stability of the PbS colloidal quantum dot film under strong electric field, high temperature, and strong light conditions, especially the high temperature stability; further, because the aluminum oxide dielectric layer has a narrow atomic spacing and is uniformly filled, the mobility of the PbS colloidal quantum dot film is improved.

[0038] In a third aspect, the optoelectronic device provided in this application adopts the following technical solution:

[0039] A photoelectric device comprises the PbS colloidal quantum dot film.

[0040] By adopting the above technical solution, PbS colloidal quantum dot films are applied to optoelectronic devices to improve the stability of optoelectronic devices.

[0041] In summary, the present application includes at least one of the following beneficial technical effects:

[0042] 1. Without destroying the surface ligands and lattice structure of the original quantum dots, reduce the content of metal-halogen compounds in the PbS colloidal quantum dot film, and fill in new dielectric layer materials to improve the stability of the PbS colloidal quantum dot film under strong electric fields, high temperatures, and strong light;

[0043] 2. Use a dielectric layer with narrower atomic spacing to replace metal-halogen compounds with poor stability under strong electric fields, high temperatures, and strong light, thereby improving the mobility of PbS colloidal quantum dot films;

[0044] 3. When preparing the colloidal quantum dot precursor film, a polar solvent system is introduced into the spin-coating liquid to promote the formation of two-dimensional perovskite precipitation and improve the removal efficiency of metal halides; on the basis of introducing the polar solvent system, pyridine derivatives are further introduced to promote the uniformity of film formation of the solution under the polar system, comprehensively improve the uniformity of subsequent alumina filling distribution, and thereby improve the stability of PbS colloidal quantum dot film under electric field, high temperature and strong light. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 is the absorption curve of the colloidal quantum dot precursor film prepared in Example 1 of the present application after different treatments;

[0046] Figure 2 is the absorption curve of the PbS colloidal quantum dot film prepared in Example 1 of the present application after different treatments;

[0047] Figure 3 is the absorption curve of the PbS colloidal quantum dot film prepared in Example 2 of the present application after different treatments;

[0048] Figure 4 is the absorption curve of the PbS colloidal quantum dot film prepared in Example 3 of the present application after different treatments;

[0049] Figure 5 is an X-ray diffraction pattern of the colloidal quantum dot precursor film prepared in Example 1 of the present application after high temperature heating;

[0050] Figure 6 is an X-ray diffraction pattern of the PbS colloidal quantum dot film prepared in Example 1 of the present application after high temperature heating;

[0051] Figure 7 is a SEM image of the colloidal quantum dot precursor film prepared in Example 1 of the present application after high temperature heating;

[0052] Figure 8 is a SEM image of the PbS colloidal quantum dot film prepared in Example 1 of the present application after high temperature heating;

[0053] Fig. 9 is the transfer characteristic curve of the colloidal quantum dot precursor film prepared in Example 1 of the present application after being treated at different temperatures;

[0054] Fig.10 is the transfer characteristic curve of the PbS colloidal quantum dot film prepared in Example 1 of the present application after being treated at different temperatures;

[0055] Fig.11 is the transfer characteristic curve of the colloidal quantum dot precursor film prepared in Example 1 of the present application after being treated in different electric fields;

[0056] Fig.12is the transfer characteristic curve of the PbS colloidal quantum dot film prepared in Example 1 of the present application after being treated in different electric fields;

[0057] Fig.13 is the transfer characteristic curve of the colloidal quantum dot precursor film prepared in Example 1 of the present application after being treated with different strong lights;

[0058] Fig.14 is the transfer characteristic curve of the PbS colloidal quantum dot film prepared in Example 1 of the present application after being treated with different strong lights;

[0059] Fig.15 is a longitudinal elemental analysis diagram of the PbS colloidal quantum dot film prepared in Example 1 of the present application;

[0060] Fig.16 This is a longitudinal elemental analysis diagram of the PbS colloidal quantum dot film prepared in Example 5 of the present application. DETAILED DESCRIPTION

[0061] In order to improve the photoelectric conversion efficiency of colloidal quantum dot devices, halogen elements are often used as ligand molecules in related technologies to achieve a good ligand passivation effect. However, the applicant found that the colloidal quantum dot precursor film obtained by colloidal quantum dot coating with metal halide as ligand exchange will decompose under the action of strong light, crystallize under the action of high temperature, and undergo ion migration under the action of strong electric field, which seriously restricts the high temperature, electric field, and radiation stability of the colloidal quantum dot device; the present application is drawn on this basis.

[0062] The present invention provides a method for preparing a PbS colloidal quantum dot film, comprising the following steps:

[0063] A1, taking a colloidal quantum dot coating film exchanged with a metal halide as a ligand to obtain a colloidal quantum dot precursor film;

[0064] A2, dispersing and dissolving the organic halide in an acetonitrile solution at a concentration of 2 to 20 mg / ml to obtain an organic halide solution;

[0065] A3, dripping an organic halide solution onto the surface of the colloidal quantum dot precursor film and covering it, letting it stand for 10-30 seconds, then discarding the excess organic halide solution, and drying to obtain a two-dimensional perovskite precipitate film;

[0066] A4, repeatedly adding acetonitrile or methanol solution to the surface of the two-dimensional perovskite precipitation film and then drying it to clean the residual organic halide solution and the two-dimensional perovskite precipitation on the two-dimensional perovskite precipitation film to obtain a clean film;

[0067] A5. Deposit aluminum oxide on the cleaned film to obtain a PbS colloidal quantum dot film.

[0068] In certain embodiments, the preparation method of the colloidal quantum dot precursor film is:

[0069] A1a, dissolving colloidal quantum dots with oleic acid (OA) as a ligand in n-octane to obtain an oleic acid quantum dot solution, wherein the size of the quantum dots is between 3 and 15 nm, the peak of the absorption spectrum curve is between 800 and 2500 nm, and the dissolution concentration of the oleic acid quantum dot solution is 5 to 20 mg / ml;

[0070] A1b, prepare a metal-halide ligand solution, specifically:

[0071] The metal-halide ligand solution can be prepared by: weighing lead iodide and lead bromide, dissolving them in N,N-dimethylformamide (DMF) solution to obtain a metal-halide ligand solution, wherein the mass volume ratio of lead iodide, lead bromide and DMF is 0.5-2g:0.01-0.5g:10ml;

[0072] The metal-halide ligand solution can also be prepared by weighing lead iodide and dissolving it in a DMF solution to obtain a metal-halide ligand solution, wherein the mass volume ratio of lead iodide to DMF is 0.5-2 g:10 ml;

[0073] A1c, filtering the oleic acid quantum dot solution into a new container, and then filtering the metal-halide ligand solution into the new container, stirring and standing for 1-5 minutes to obtain a metal-halide exchange solution, wherein the volume ratio of the oleic acid quantum dot solution to the metal-halide ligand solution is 1:1;

[0074] A1d, purifying the metal-halide exchange liquid to obtain colloidal quantum dots exchanged with metal halides as ligands, specifically:

[0075] The metal-halide exchange solution is allowed to stand for stratification, the upper clear liquid is discarded, the n-octane solution is added, and the solution is shaken or stirred again, and the solution is allowed to stand for 3-5 minutes. This step is repeated at least twice to obtain the lead sulfide quantum dot solution after the lower layer exchange, and the solution is centrifuged and dried to obtain colloidal quantum dots (powder) exchanged with metal halides as ligands;

[0076] A1e, dissolving the colloidal quantum dots exchanged with metal halide as ligands with a spin coating liquid to obtain a slurry, the dissolution concentration of which is 100-500 mg / ml, wherein the spin coating liquid can be an amine low boiling point solvent, and the amine low boiling point solvent can be at least one of n-butylamine, n-hexylamine, and n-pentylamine;

[0077] A1f, spin-coating the slurry on the surface of a glass or silicon wafer substrate at a rotation speed of 2000rpm-5000rpm, and then placing the glass or silicon wafer substrate after spin-coating the slurry on a hot plate at a temperature between 50-150°C for annealing and drying, and finally obtaining a colloidal quantum dot precursor film.

[0078] In some embodiments, the spin coating liquid can also be a mixture of a polar organic solvent and an amine low boiling point solvent, the volume ratio of the polar organic solvent to the amine low boiling point solvent is 1-4:1, and the polar organic solvent can be at least one of strong polar solvents such as N,N-dimethylformamide and dimethyl sulfoxide.

[0079] In some embodiments, the spin-coating liquid can also be a mixture of a polar organic solvent, an amine low-boiling point solvent, and a pyridine derivative, wherein the pyridine derivative accounts for 0.1-5% of the total volume of the spin-coating liquid. The pyridine derivative can specifically be at least one of aminomethylpyridine, aminopyridine, and pyridine.

[0080] In certain embodiments, the organic halide may be at least one of phenethylammonium iodide, methylamine iodide, p-fluorophenethylammonium iodide, phenethylammonium bromide, and fluoroethylammonium bromide.

[0081] In some embodiments, depositing aluminum oxide on the cleaning film is specifically:

[0082] The cleaned film is placed in an atomic layer deposition (ALD) chamber, and alkyl aluminum (specifically trimethyl aluminum) and an oxygen source (specifically one of water and ozone) are used as precursor raw materials. A pulse time of 0.1 s and a cleaning (purge) time of 10-100 s are used to grow the film for 5-30 cycles, and finally a PbS colloidal quantum dot film is obtained.

[0083] Furthermore, the embodiments of the present application provide a PbS colloidal quantum dot film, and a photoelectric device including the PbS colloidal quantum dot film. The photoelectric device may specifically be a solar cell, a photodetector, a light emitting diode, or a transistor.

[0084] The present application is further described in detail below in conjunction with embodiments.

[0085] Embodiment 1:

[0086] A method for preparing a PbS colloidal quantum dot film comprises the following steps:

[0087] S1, taking a colloidal quantum dot coating film exchanged with a metal halide as a ligand to obtain a colloidal quantum dot precursor film;

[0088] Wherein, the preparation method of colloidal quantum dot precursor film is:

[0089] S1a, dissolving colloidal quantum dots with oleic acid (OA) as a ligand in n-octane to obtain an oleic acid quantum dot solution, wherein the dissolution concentration of the oleic acid quantum dot solution is 10 mg / ml;

[0090] S1b, prepare a metal-halide ligand solution, specifically:

[0091] The metal-halide ligand solution can be prepared by weighing 1.2 g of lead iodide and 0.4 g of lead bromide, dissolving them in 10 ml of N,N-dimethylformamide (DMF) solution to obtain a metal-halide ligand solution;

[0092] S1c, filter 10 ml of the oleic acid quantum dot solution into a new container, and then filter 10 ml of the metal-halide ligand solution into the new container, stir and let stand for 3 minutes to obtain a metal-halide exchange solution;

[0093] S1d, purifying the metal-halide exchange liquid to obtain colloidal quantum dots exchanged with metal halides as ligands, specifically:

[0094] The metal-halide exchange solution was allowed to stand for stratification, the upper clear liquid was discarded, the n-octane solution was added, and the mixture was stirred evenly again, and the mixture was allowed to stand for 4 minutes. This step was repeated twice to obtain the lead sulfide quantum dot solution after the lower layer exchange, and the solution was centrifuged and dried to obtain colloidal quantum dots (powder) exchanged with metal halides as ligands;

[0095] S1e, dissolving the colloidal quantum dots exchanged with metal halide as ligands with a spin coating liquid to obtain a slurry, the dissolution concentration is 400 mg / ml, wherein: the spin coating liquid is N, N-dimethylformamide and n-butylamine in a volume ratio of 5:3;

[0096] S1f, spin-coating the slurry on the surface of a glass or silicon wafer substrate at a rotation speed of 2500 rpm, and then placing the glass or silicon wafer substrate after spin-coating the slurry on a hot plate at a temperature of 90° C. for annealing and drying, and finally obtaining a colloidal quantum dot precursor film.

[0097] S2, dispersing and dissolving phenethylammonium iodide (PEAI) in an acetonitrile solution at a concentration of 5 mg / ml to obtain an organic halide solution;

[0098] S3, dripping an organic halide solution onto the surface of the colloidal quantum dot precursor film and covering it, letting it stand for 20 seconds, then discarding the excess organic halide solution, and drying to obtain a two-dimensional perovskite precipitate film;

[0099] S4, dropping acetonitrile solution on the surface of the two-dimensional perovskite precipitation film twice and then spinning to clean the residual organic halide solution and the two-dimensional perovskite precipitation on the two-dimensional perovskite precipitation film to obtain a cleaned film;

[0100] S5. Place the cleaned film in an atomic layer deposition (ALD) chamber, use trimethylaluminum and water as precursor materials, grow for 20 cycles with a pulse time of 0.1 s and a cleaning (purge) time of 50 s to deposit aluminum oxide on the cleaned film to obtain a PbS colloidal quantum dot film.

[0101] Example 2

[0102] A method for preparing a PbS colloidal quantum dot film comprises the following steps:

[0103] S1, taking a colloidal quantum dot coating film exchanged with a metal halide as a ligand to obtain a colloidal quantum dot precursor film;

[0104] Wherein, the preparation method of colloidal quantum dot precursor film is:

[0105] S1a, dissolving colloidal quantum dots with oleic acid (OA) as a ligand in n-octane to obtain an oleic acid quantum dot solution, wherein the concentration of the oleic acid quantum dot solution is 5 mg / ml;

[0106] S1b, prepare a metal-halide ligand solution, specifically:

[0107] The metal-halide ligand solution can be prepared by weighing 0.5 g of lead iodide and 0.2 g of lead bromide, and dissolving them in 10 ml of N,N-dimethylformamide (DMF) solution to obtain a metal-halide ligand solution;

[0108] S1c, filtering the oleic acid quantum dot solution into a new container, and then filtering the metal-halide ligand solution into the new container, stirring and standing for 3 minutes to obtain a metal-halide exchange solution, wherein the volume ratio of the oleic acid quantum dot solution to the metal-halide ligand solution is 1:1;

[0109] S1d, purifying the metal-halide exchange liquid to obtain colloidal quantum dots exchanged with metal halides as ligands, specifically:

[0110] The metal-halide exchange solution is allowed to stand for stratification, the upper clear liquid is discarded, the n-octane solution is added, and the solution is shaken or stirred again, and the solution is allowed to stand for 5 minutes. This step is repeated twice to obtain the lead sulfide quantum dot solution after the lower layer exchange, and the solution is centrifuged and dried to obtain colloidal quantum dots (powder) exchanged with metal halides as ligands;

[0111] S1e, dissolving the colloidal quantum dots exchanged with metal halide as ligands with a spin coating liquid to obtain a slurry, the dissolution concentration is 100 mg / ml, wherein: the spin coating liquid is N, N-dimethylformamide and n-butylamine in a volume ratio of 1:1;

[0112] S1f, spin-coating the slurry on the surface of a glass or silicon wafer substrate at a rotation speed of 2000 rpm, and then placing the glass or silicon wafer substrate after spin-coating the slurry on a hot plate at a temperature of 50° C. for annealing and drying, and finally obtaining a colloidal quantum dot precursor film.

[0113] S2, dispersing and dissolving the organic halide in the acetonitrile solution at a concentration of 2 mg / ml to obtain an organic halide solution, wherein the organic halide is p-fluorophenethylammonium iodide;

[0114] S3, dripping an organic halide solution onto the surface of the colloidal quantum dot precursor film to cover it, letting it stand for 10 seconds, then throwing out the excess organic halide solution, and drying to obtain a two-dimensional perovskite precipitate film;

[0115] S4, adding acetonitrile solution dropwise onto the surface of the two-dimensional perovskite precipitate film three times and then spinning to clean the residual organic halide solution and the two-dimensional perovskite precipitate on the two-dimensional perovskite precipitate film to obtain a cleaned film;

[0116] S5. Place the cleaned film in an atomic layer deposition (ALD) chamber, use trimethylaluminum and water as precursor materials, grow for 20 cycles with a pulse time of 0.1 s and a cleaning (purge) time of 50 s to deposit aluminum oxide on the cleaned film to obtain a PbS colloidal quantum dot film.

[0117] Example 3

[0118] A method for preparing a PbS colloidal quantum dot film comprises the following steps:

[0119] S1, taking a colloidal quantum dot coating film exchanged with a metal halide as a ligand to obtain a colloidal quantum dot precursor film;

[0120] Wherein, the preparation method of colloidal quantum dot precursor film is:

[0121] S1a, dissolving colloidal quantum dots with oleic acid (OA) as a ligand in n-octane to obtain an oleic acid quantum dot solution, wherein the dissolution concentration of the oleic acid quantum dot solution is 20 mg / ml;

[0122] S1b, prepare a metal-halide ligand solution, specifically:

[0123] The metal-halide ligand solution can be prepared by weighing 2 g of lead iodide and 0.5 g of lead bromide and dissolving them in 10 ml of N,N-dimethylformamide (DMF) solution to obtain a metal-halide ligand solution;

[0124] S1c, filtering the oleic acid quantum dot solution into a new container, and then filtering the metal-halide ligand solution into the new container, stirring and standing for 3 minutes to obtain a metal-halide exchange solution, wherein the volume ratio of the oleic acid quantum dot solution to the metal-halide ligand solution is 1:1;

[0125] S1d, purifying the metal-halide exchange liquid to obtain colloidal quantum dots exchanged with metal halides as ligands, specifically:

[0126] The metal-halide exchange solution is allowed to stand for stratification, the upper clear liquid is discarded, the n-octane solution is added, and the solution is shaken or stirred again, and the solution is allowed to stand for 3 minutes. This step is repeated three times to obtain the lead sulfide quantum dot solution after the lower layer exchange, and the solution is centrifuged and dried to obtain colloidal quantum dots (powder) exchanged with metal halides as ligands;

[0127] S1e, dissolving the colloidal quantum dots exchanged with metal halide as ligands with a spin coating liquid to obtain a slurry, the dissolution concentration of which is 100-500 mg / ml, wherein the spin coating liquid can be an amine low boiling point solvent, and the amine low boiling point solvent can be at least one of n-butylamine, n-hexylamine, and n-pentylamine;

[0128] S1f, spin-coating the slurry on the surface of a glass or silicon wafer substrate at a rotation speed of 5000 rpm, and then placing the glass or silicon wafer substrate after the slurry is spin-coated on a hot plate at a temperature between 50-150° C. for annealing and drying, and finally obtaining a colloidal quantum dot precursor film.

[0129] S2, dispersing and dissolving the organic halide in the acetonitrile solution at a concentration of 20 mg / ml to obtain an organic halide solution, wherein the organic halide is at least one of phenethylammonium iodide, methylamine iodide, p-fluorophenethylammonium iodide, phenethylammonium bromide, and fluoroethylammonium bromide;

[0130] S3, dripping an organic halide solution onto the surface of the colloidal quantum dot precursor film to cover it, letting it stand for 30 seconds, then throwing out the excess organic halide solution, and drying to obtain a two-dimensional perovskite precipitate film;

[0131] S4, adding methanol solution dropwise twice onto the surface of the two-dimensional perovskite precipitate film and then spinning to clean the residual organic halide solution and the two-dimensional perovskite precipitate on the two-dimensional perovskite precipitate film to obtain a cleaned film;

[0132] S5. Place the cleaned film in an atomic layer deposition (ALD) chamber, use trimethylaluminum and water as precursor materials, grow for 20 cycles with a pulse time of 0.1 s and a cleaning (purge) time of 50 s to deposit aluminum oxide on the cleaned film to obtain a PbS colloidal quantum dot film.

[0133] Embodiment 4:

[0134] A method for preparing a PbS colloidal quantum dot film is the same as that of Example 1, except that the spin coating liquid is n-butylamine.

[0135] Embodiment 5:

[0136] A method for preparing a PbS colloidal quantum dot film is the same as that of Example 1, except that the spin coating liquid further comprises aminomethylpyridine, and the aminomethylpyridine accounts for 3% of the total volume of the spin coating liquid.

[0137] test

[0138] 1. Stability test

[0139] 1.1. High temperature stability

[0140] 1.1.1 Absorption curve characterization

[0141] The colloidal quantum dot precursor film and PbS colloidal quantum dot film prepared in Example 1, the PbS colloidal quantum dot film prepared in Example 2, and the PbS colloidal quantum dot film prepared in Example 3 were respectively subjected to no treatment (initial), heating at 120°C for 11h, and heating at 220°C for 60h to obtain 12 samples to be tested. The absorption curves of the samples to be tested were characterized respectively. The characterization results were referred to Figure 1-4 As shown:

[0142] Figure 1 The absorption spectra of the colloidal quantum dot precursor film prepared in Example 1 after different treatments are shown in FIG. Figure 1 It can be seen that in the initial state, the colloidal quantum dot precursor film has an obvious exciton absorption peak reflecting the characteristics of quantum dots. After being heated at 120℃ for 11h, the absorption peak has a significant change, and after being heated at 220℃ for 60h, the exciton absorption peak reflecting the characteristics of quantum dots basically disappears completely, indicating that its high temperature stability is poor.

[0143] Figure 2 The absorption spectra of the PbS colloidal quantum dot film prepared in Example 1 after different treatments are shown in FIG. Figure 2 It can be seen that the PbS colloidal quantum dot film prepared in Example 1 has no obvious change in absorption peak between the initial state and after being heated at 120°C for 11h. Even after being heated at 220°C for 60h, it still has obvious exciton absorption peaks reflecting the characteristics of quantum dots compared to the initial state, indicating that it has excellent high temperature stability.

[0144] Figure 3 The absorption spectra of the PbS colloidal quantum dot film prepared in Example 2 after different treatments are shown below. Figure 4 The absorption spectra of the PbS colloidal quantum dot film prepared in Example 3 after different treatments are shown in FIG. Figure 3 , 4 It can be seen that the PbS colloidal quantum dot films prepared in Example 2 and Example 3 also have excellent high-temperature stability.

[0145] 1.1.2 X-ray diffraction characterization

[0146] The colloidal quantum dot precursor film and the PbS colloidal quantum dot film prepared in Example 1 were characterized by X-ray diffraction in the initial state and after being heated at 220°C for 60h. The characterization results are shown in Table 1. Figure 5-6 As shown:

[0147] Figure 5 The X-ray diffraction characterization results of the colloidal quantum dot precursor film prepared in Example 1 in the initial state and after being heated at 220°C for 60 hours are compared with the lead sulfide standard card (PbS-PDF) and the lead iodide standard card (PbI 2 -PDF), Lead Bromide Standard Card (PbBr 2 -PDF) comparison shows that there are no impurity peaks related to lead halides in the initial state, but many impurity peaks related to lead halides are formed after high temperature treatment;

[0148] Figure 6 The X-ray diffraction characterization results of the PbS colloidal quantum dot film prepared in Example 1 after heating at 220°C for 60h are compared with the lead sulfide standard card (PbS-PDF) and the lead iodide standard card (PbI 2 -PDF), Lead Bromide Standard Card (PbBr 2 -PDF) comparison shows that, after high temperature treatment, the PbS crystal peak position is still relatively pure and consistent with the initial state.

[0149] 1.1.3 SEM characterization

[0150] The colloidal quantum dot precursor film and the PbS colloidal quantum dot film prepared in Example 1 were heated at 220°C for 60 hours and then characterized by SEM. The characterization results are shown in Table 1. Figure 7-8 As shown:

[0151] Figure 7 This is a SEM image of the colloidal quantum dot precursor film prepared in Example 1 after being heated at 220°C for 60 hours. Figure 7 It can be seen that after high-temperature treatment, many fine grains and protrusions appear on the surface of the film due to the crystallization of metal halides at high temperatures;

[0152] Figure 8 This is a SEM image of the PbS colloidal quantum dot film prepared in Example 1 after being heated at 220°C for 60 hours. Figure 8 It can be seen that after high-temperature treatment, the surface morphology of the PbS colloidal quantum dot film is always good without the appearance of fine grains or protrusions.

[0153] 1.1.4 Field Effect Transistor Characterization

[0154] The transfer characteristic curves (V gate -I drain ) for characterization, and the characterization results refer to Figure 9-10 As shown:

[0155] Fig. 9 The transfer characteristic curve (V gate -I drain ),Depend on Fig. 9 It can be seen that after high temperature treatment, the drain current (I drain ) has increased by more than one order of magnitude, and the modulation characteristics of the field effect tube have been lost;

[0156] Fig.10 The transfer characteristic curve (V gate -I drain ),Depend on Fig.10 It can be seen that after high temperature treatment, the drain current (I drain ).

[0157] 1.2. High electric field stability

[0158] The colloidal quantum dot precursor film and the PbS colloidal quantum dot film prepared in Example 1 were respectively subjected to no treatment (before aging) and high electric field treatment of 200,000 volts per meter for 87 hours (after aging) to obtain four samples to be tested. The transfer characteristic curves (V gate -I drain ) characterization, characterization results refer to Figure 11-12 As shown:

[0159] Fig.11 The transfer characteristic curves (V gate -I drain ),Depend on Fig.11 It can be seen that the drain current (I drain ) has increased by more than one order of magnitude, and the modulation characteristics of the field effect tube have been lost, resulting in a huge hysteresis effect, indicating that its high electric field stability is poor;

[0160] Fig.12 The transfer characteristic curves (V gate -I drain ),Depend on Fig.12It can be seen that the PbS colloidal quantum dot film prepared in Example 1 still has a drain current (I drain ), indicating that it has excellent high electric field stability.

[0161] 1.3. Strong light stability

[0162] The colloidal quantum dot precursor film and the PbS colloidal quantum dot film prepared in Example 1 were taken without treatment (before aging) and irradiated with strong light of AM1.5 for 55 hours (after aging) to obtain 4 samples to be tested. The transfer characteristic curves (V gate -I drain ) characterization, characterization results refer to Figure 13-14 As shown:

[0163] Fig.13 The transfer characteristic curve (V gate -I drain ),Depend on Fig.13 It can be seen that the drain current (I drain ) increased by more than 3 times, indicating that its strong light stability is poor;

[0164] Fig.14 The transfer characteristic curves (V gate -I drain ),Depend on Fig.14 It can be seen that the drain current of the PbS colloidal quantum dot film prepared in Example 1 is basically at the same level after 55 hours of strong light irradiation, indicating that it has better strong light stability.

[0165] 2. Time-of-Flight Secondary Ion Mass Spectrometry TOF-SIMS Characterization

[0166] In time-of-flight secondary ion mass spectrometry, a low-energy ion beam is applied to the sample, which etches the sample to form a tiny sputtering pit. At the same time, a pulsed ion beam is used to analyze the center of the sputtering pit to obtain a longitudinal elemental analysis diagram of the sample.

[0167] The PbS colloidal quantum dot films prepared in Example 1 and Example 5 were respectively subjected to longitudinal element analysis using a time-of-flight secondary ion mass spectrometer TOF-SIMS instrument. The test results are as follows: Figure 15-16 As shown, for each figure, from the left to the right, it represents the distribution of elements from the surface layer to the inner layer in the film;

[0168] Fig.15This is a longitudinal elemental analysis diagram of the PbS colloidal quantum dot film prepared in Example 1. Fig.15 It can be seen that Al 2+ The content of elements decreases gradually from left to right, indicating that aluminum oxide (Al 2 O 3 ) lack of uniform distribution in PbS colloidal quantum dot films;

[0169] Fig.16 This is a longitudinal elemental analysis diagram of the PbS colloidal quantum dot film prepared in Example 2. Fig.16 It can be seen that Al 2+ The content of elements shows a horizontal trend from left to right, indicating that aluminum oxide (Al 2 O 3 ) are evenly distributed in the PbS colloidal quantum dot film.

[0170] The embodiments of this specific implementation are all preferred embodiments of the present application, and are not intended to limit the protection scope of the present application. The same components are represented by the same figure marks. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A method for preparing a PbS colloidal quantum dot film, characterized in that: The following steps are involved: Taking a colloidal quantum dot coating film exchanged with a metal halide as a ligand to obtain a colloidal quantum dot precursor film; dispersing and dissolving an organic halide to obtain an organic halide solution; Add an organic halide solution dropwise onto the surface of the colloidal quantum dot precursor film to cover it, shake off excess organic halide solution after standing, and dry to obtain a two-dimensional perovskite precipitate film; cleaning the residual organic halide solution and the two-dimensional perovskite precipitate on the two-dimensional perovskite precipitate film to obtain a cleaned film; Aluminum oxide is deposited on the cleaned film to obtain a PbS colloidal quantum dot film.

2. The method for preparing a PbS colloidal quantum dot thin film according to claim 1, characterized in that: The preparation method of the colloidal quantum dot precursor film is as follows: Taking colloidal quantum dots with oleic acid as ligand and dissolving them in n-octane to obtain an oleic acid quantum dot solution; preparing a metal-halide ligand solution; Adding the oleic acid quantum dot solution to the metal-halide ligand solution, stirring and then standing to obtain a metal-halide exchange solution; Purifying the metal-halide exchange solution to obtain colloidal quantum dots using metal halides as ligands for exchange; The colloidal quantum dots exchanged with metal halide as ligand are dissolved in a spin coating liquid to obtain a slurry, wherein the spin coating liquid is an amine low boiling point solvent; The slurry is spin-coated on the surface of the substrate to obtain a colloidal quantum dot precursor film.

3. The method for preparing a PbS colloidal quantum dot thin film according to claim 2, characterized in that: The spin coating liquid also includes a polar organic solvent, and the volume ratio of the polar organic solvent to the amine low boiling point solvent is 1-4:

1.

4. The method for preparing a PbS colloidal quantum dot thin film according to claim 3, characterized in that: The polar organic solvent is at least one of N,N-dimethylformamide and dimethyl sulfoxide.

5. The method for preparing a PbS colloidal quantum dot thin film according to claim 3, characterized in that: The spin coating liquid also includes pyridine derivatives, and the pyridine derivatives account for 0.1-5% of the total volume of the spin coating liquid.

6. The method for preparing a PbS colloidal quantum dot thin film according to claim 1, characterized in that: The residual organic halide solution and the two-dimensional perovskite precipitate on the two-dimensional perovskite precipitate film are cleaned, specifically, by repeatedly dropping acetonitrile or methanol solution on the surface of the two-dimensional perovskite precipitate film and then drying it.

7. The method for preparing a PbS colloidal quantum dot thin film according to claim 1, characterized in that: The organic halide is at least one of phenethylammonium iodide, methylamine iodide, p-fluorophenethylammonium iodide, phenethylammonium bromide, and fluoroethylammonium bromide.

8. The method for preparing a PbS colloidal quantum dot thin film according to claim 5, characterized in that: The aluminum oxide is deposited on the cleaned film by using trimethylaluminum and water as precursor raw materials, and growing for 5 to 30 cycles with a pulse time of 0.1 s and a purge time of 10 to 100 s.

9. PbS colloidal quantum dot film, characterized in that: The film is prepared by the method for preparing a PbS colloidal quantum dot film as described in any one of claims 1 to 8.

10. An optoelectronic device, characterized in that Comprising the PbS colloidal quantum dot film as described in claim 9.