Method for comprehensively recovering various valuable components from red mud

Through activation and water immersion treatment of red mud, combined with multi-stage extraction and precipitation technology, high-efficiency aluminum-ferrous composite flocculants, high-purity vanadium pentoxide and scandium trioxide were prepared, which solved the problem of red mud in the prior art. The singularity and high consumption problems of the valent metal recycling process have achieved efficient recycling of a variety of valuable components and high value-added products.

CN119061256APending Publication Date: 2024-12-03HENAN POLYTECHNIC UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411107033.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing valuable metal recycling process in red mud has problems such as single recycling method, high chemical consumption in leaching and decaling process, single leaching liquid composition, high temperature and complex process, especially when combined recycling of vanadium, scandium, titanium, silicon, aluminum, etc. There are problems such as limited recovery rate, high cost, tailings and waste liquid emissions.

Method used

Using activated roasting-water immersion, reselection, complexing-extraction, fractionated stripping-precipitation-calcination, modified starch polymerization of iron aluminum, red mud is treated through activated roasting, combined with water immersion and reselection, and DTPA complexing is used. The agent and P507 extractant were carried out for multi-stage extraction and precipitation, and finally, through modified starch polymerization, iron aluminum-ferrous aluminum composite flocculant, vanadium pentoxide and scandium trioxide and other products were prepared.

Benefits of technology

It has achieved efficient recycling of a variety of valuable components, including high recovery rates and high purity products of aluminum, iron, vanadium, scandium, avoided the discharge of tailings and waste liquids, and improved the added value and comprehensive utilization prospects of recycled products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061256A_ABST
    Figure CN119061256A_ABST
Patent Text Reader

Abstract

The invention discloses a method for comprehensively recovering various valuable components from red mud, and relates to the field of red mud treatment. The method comprises the following steps: firstly, mixing red mud with sulfuric acid, performing low-temperature activated roasting, and performing water leaching on activated roasting clinker to obtain a leaching solution containing valuable metal ions such as aluminum, iron, vanadium and scandium and leaching residues containing anhydrite and white carbon black; leached residues are separated through a shaking table to obtain high-grade anhydrite concentrate and white carbon black concentrate, and after leaching liquid is subjected to complexing extraction, vanadium and scandium are enriched in a loaded organic phase, and aluminum and iron are left in raffinate; the loaded organic phase is subjected to two-stage reverse extraction, precipitation and calcination to obtain high-purity vanadium pentoxide and scandium trioxide, and raffinate containing aluminum and iron is polymerized through modified starch to prepare the composite flocculant with the total content of aluminum ferric sulfate larger than 75%. The method provided by the invention can comprehensively recover valuable components of red mud, and has the advantages of multiple types of recovered valuable components, high recovery rate, high additional value of recovered products, no discharge of tailings and waste liquid, and wide comprehensive utilization prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of comprehensive red mud treatment, and in particular to a method for comprehensively recovering multiple valuable components from red mud. Background Art

[0002] Red mud is a highly alkaline waste residue discharged during the smelting of alumina from bauxite. For every ton of alumina produced, 1.0 to 2.0 tons of red mud will be produced. my country's annual red mud production is 107 million tons, and the total stockpile has exceeded 1.1 billion tons, covering an area of ​​more than 120,000 mu (enough to fill about 60 West Lakes). The total stockpile rate is 95%, and it is mainly disposed of by damming and stockpiling, with a comprehensive utilization rate of less than 6% (see: Zhang J, Yao Z, Wang K, et al. Sustainable utilization of bauxite residue (Red Mud) as a road material in pavements: a critical review [J]. Construction and Building Materials, 2021, 270: 121419.).

[0003] Red mud is rich in a variety of useful components and can be fully utilized in many fields. The comprehensive utilization of red mud includes the preparation of building materials, soil resource utilization and recovery of valuable components (Wang Yaguang. Microstructure evolution and composite synergistic effect of new cementitious materials of red mud-fly ash-desulfurized gypsum [D], Beijing University of Science and Technology. 2022). However, due to the strong alkalinity of red mud, many problems need to be solved in its production of building materials and soil resource utilization, such as alkali blooming and frost in red mud-based building materials, and soil salinization in the process of soil resource utilization. At the same time, since the main components of red mud include aluminum oxide, iron oxide, silicon dioxide, calcium oxide, etc., and it also contains rare metals such as scandium trioxide and vanadium pentoxide, it can be recycled as valuable components. Regarding the recovery of valuable metals, the current process of magnetization roasting-magnetic separation is used to recover iron, and the process of alkali roasting-alkali leaching is used to recover aluminum (Dong Hongjun, Chen Chang. Research on flash magnetization roasting technology of red mud [J]. Mining and Metallurgical Engineering, 2022, 42(06): 142-145; Li Bin, Wang Zhiping, Qu Fan, et al. Current status and prospects of recovery of valuable metals in red mud [J]. Journal of Kunming University of Science and Technology (Natural Science Edition), 2019, 44(02): 1-10). The above-mentioned recovery processes of valuable metals, represented by the recovery of aluminum or iron, have the disadvantages of relatively simple recovery methods of valuable components in red mud, high consumption of reagents in the leaching and dealkalization process, single recovery components of valuable metals such as vanadium, aluminum, and iron in the leaching solution, high leaching temperature, and complex process.

[0004] In addition to the above-mentioned separate recovery processes for valuable metals, there are now also processes for the combined recovery of aluminum and iron. The most representative of these is the wet acid leaching process. With its advantages of high leaching rate and low cost, wet acid leaching has become an effective method for the combined recovery of aluminum and iron. At the same time, red mud acid leaching liquid contains a large amount of aluminum and iron, which can be used to prepare aluminum-iron based polymer flocculants (Yuan Xiaoxiao, Xia Yuxin, Li Jia, et al. Research and Application of Red Mud Based Environmental Remediation Materials [J]. Journal of Hubei University of Technology, 2020, 36(06):15-18+56; Qian Yi, Zhou Shaojie. Preparation of Red Mud Based Polyaluminum Ferric Sulfate and Evaluation of Its Flocculation Performance [J]. Environmental Engineering, 2016, 34(08):6-10.). The flocculant prepared using red mud acid leaching liquid can not only alleviate the red mud storage problem but also achieve various wastewater treatments. In addition, the valuable metals such as aluminum and iron recovered by red mud acid leaching and the product flocculants prepared using the recovered aluminum and iron will not be affected by the alkalinity of red mud in subsequent use.

[0005] In summary, compared with the traditional separate recovery process of aluminum or iron, the current wet acid leaching process is an effective and mature process for the joint recovery of aluminum and iron. It has the advantages of simultaneously recovering two valuable metals, aluminum and iron, high leaching rate, low cost, and the recovered valuable metals and flocculants are not affected by the alkalinity of red mud in subsequent use. Although the current wet acid leaching process has an enlightening effect on the joint recovery of other valuable metals such as vanadium, scandium, titanium, silicon, and aluminum, there are problems such as different types of leaching acids corresponding to different recovery components, limited leaching rate and recovery rate, high cost, tailings and waste liquid discharge when recovering other valuable metals such as vanadium, scandium, titanium, silicon, and aluminum. Therefore, it is necessary to further improve and optimize the current wet acid leaching process, and provide a method for comprehensive recovery of multiple valuable components from red mud with multiple types of valuable components, high recovery rate, high added value of recovered products, no tailings and waste liquid discharge, and broad prospects for comprehensive utilization. Summary of the invention

[0006] The purpose of the present invention is to provide a method for comprehensive recovery of multiple valuable components from red mud in view of the deficiencies in the above-mentioned prior art. The present invention adopts the technology of activated roasting-water leaching, gravity separation, complexation-extraction, graded stripping-precipitation-calcination, and modified starch polymerization of aluminum and iron to comprehensively recover the valuable components of red mud, and obtains multiple valuable products such as aluminum-iron composite flocculant, vanadium pentoxide, scandium trioxide, anhydrite and white carbon black, which has the advantages of multiple types of valuable component recovery, high recovery rate, high added value of recovered products, no tailings and waste liquid discharge, and broad prospects for comprehensive utilization.

[0007] The purpose of the present invention can be achieved by the following technical measures: A method for comprehensively recovering multiple valuable components from red mud of the present invention is to adopt the technology of activated roasting-water leaching, gravity separation, complexation-extraction, graded stripping-precipitation-calcination, and modified starch polymerization of aluminum and iron to comprehensively recover the valuable components of red mud, and finally obtain aluminum-iron composite flocculant, vanadium pentoxide, scandium trioxide, anhydrite and white carbon black, and the specific steps are as follows: a. Red mud activation roasting-water immersion In the activation roasting process, the red mud raw material and sulfuric acid are evenly mixed in a mass ratio of 10:1-3, and then the mixture is placed in an electric furnace with a heating rate of 10°C / min, and roasted at a roasting temperature of 200-300°C for 30-90min; after roasting and cooling, the roasted sample is mixed with deionized water in a mass ratio of 1:5-10, and stirred at a leaching temperature of 30-90°C for 60-120min. After the leaching is completed, the leachate and the leaching residue are obtained by solid-liquid separation; b. Separation of anhydrite and white carbon black by gravity separation of leaching residue The leached residue obtained in step a is subjected to gravity separation, and the specific process is to use a shaking table as a gravity separation device, and to obtain two products, anhydrite and white carbon black, through 2-3 levels of shaking table separation under the separation conditions of a stroke of 8-36 mm, a stroke of 240-380 times / min, a bed surface transverse slope of 0-10°, and a separation particle size of 0.01-1 mm; c. Separation and purification of rare and precious metals in the leaching solution The leaching solution obtained in step a is pre-complexed, specifically, the pH value of the leaching solution is adjusted to 1.0-2.0 with 1 mol / L NaOH and 1 mol / L H2SO4, and then a DTPA complexing agent is added at a solid-liquid mass ratio of 1-3:10 and stirred evenly as an extraction liquid phase, and the extraction is performed at a volume ratio of the extraction liquid phase to the organic phase of 1-3:1 for 5-8 minutes, and static stratification is performed for 3-5 minutes to obtain a raffinate and a loaded organic phase; the loaded organic phase is subjected to two-stage stripping, precipitation and calcination to obtain vanadium pentoxide and scandium trioxide, and the organic phase is reused after regeneration; d. Modified polymerization of aluminum / iron in the raffinate The raffinate obtained in step c is polymerized and aged, the polymerization temperature is set to 30-50°C, and the mass ratio m is (Al+Fe) :m 淀粉 Aluminum sulfate, ferric sulfate and modified starch are added to the raffinate in a ratio of 100:1-10 in sequence, and sodium hydroxide solution is added while stirring to adjust the pH value of the raffinate to 2.5-3.5. After stirring, the raffinate is aged for 6-24 hours, and finally spray-dried to obtain an aluminum-iron composite flocculant.

[0008] The red mud of the present invention has an aluminum oxide content of 10% to 40%, an iron oxide content of 5 to 20%, a silicon dioxide content of 20 to 40%, a vanadium pentoxide content of 0.05 to 0.6%, and a scandium trioxide content of 0.002 to 0.01%.

[0009] The anhydrite and white carbon black described in the present invention are products formed after the red mud is activated and roasted by sulphation. The anhydrite and white carbon black are insoluble in water during the water leaching process and exist in the leached residue. After gravity separation, the grade of anhydrite is greater than 92%, and the grade of white carbon black is greater than 95%.

[0010] The organic phase of the present invention is composed of P507 as the main extractant and sulfonated kerosene as the diluent; the process of two-stage stripping, precipitation and calcination: first, the loaded organic phase and 2-4 mol / L sulfuric acid solution are mixed according to a volume ratio of 10:1-5 and shaken for 5-10 minutes, and static stratification is performed for 3-5 minutes to obtain vanadium-rich liquid and scandium-rich organic phase; then, the scandium-rich organic phase is mixed with 2-4 mol / L sodium hydroxide solution according to a volume ratio of 10:1-5 and shaken for 5-10 minutes, and static stratification is performed for 3-5 minutes. n, a crude scandium hydroxide product and a regenerated organic phase are obtained; the vanadium-rich solution is subjected to an acidic ammonium salt precipitation method to obtain a polyammonium vanadate precipitate, and the precipitate is calcined at 450-500°C for 40-60min to obtain vanadium pentoxide; the crude scandium hydroxide product is dissolved in sulfuric acid and precipitated with oxalic acid to obtain a scandium oxalate precipitate, and the precipitate is washed with three levels of water and calcined at 500-600°C for 20-30min to obtain scandium trioxide; the regenerated organic phase is rinsed with a 1-3 mol / L hydrochloric acid solution for 3-5 times and can be continuously used for extraction operations.

[0011] The purity of the vanadium pentoxide product in the present invention is greater than 99.5%, and the purity of the scandium trioxide product is greater than 99.1%.

[0012] The modified starch described in the present invention is prepared by chemically modifying corn starch through etherification.

[0013] The vanadium concentration in the raffinate of the present invention is less than 3 ppm, the scandium concentration is less than 0.1 ppm, the aluminum content is greater than 5 g / L, and the iron content is greater than 3 g / L.

[0014] The total content of aluminum sulfate and iron in the aluminum-iron composite flocculant of the present invention is greater than 75%, and the flocculant belongs to an organic / inorganic composite material.

[0015] The design principle of the present invention is as follows: The invention adopts the technology of activated roasting-water leaching, gravity separation, complexation-extraction, graded stripping-precipitation-calcination and modified starch polymerization of aluminum and iron to comprehensively recover the valuable components of red mud, and obtain various valuable products such as aluminum-iron composite flocculant, vanadium pentoxide, scandium trioxide, anhydrite and white carbon black.

[0016] Since the red mud contains high aluminum and iron content and is not easy to be leached and recovered, the sulfuric acid roasting technology is used for activation treatment. Figure 1 ( Figure 1 It is composed of four sub-graphs: Figure 1 a. points Figure 1 b. Points Figure 1 c. points Figure 1 d).

[0017] As the roasting temperature increases, the leaching rate of the two elements increases; when the roasting temperature is close to 250℃, the leaching rate increases; when the roasting temperature exceeds 250℃, the leaching rate decreases with the increase of temperature. Figure 1 As shown in a. At 350°C, the leaching rate of iron is halved. According to the results of thermodynamic research, high temperature has no significant promoting effect on iron leaching. When the temperature exceeds 250°C, a certain amount of sulfuric acid evaporates, resulting in insufficient sulfuric acid in the reaction system, affecting the reaction process, which is the main reason for the sudden and sharp drop in the leaching rate. Figure 1 b shows the effect of roasting time on the leaching rates of aluminum and iron. When the roasting time is 1h, the aluminum leaching rate tends to be stable, and as the roasting time increases, its leaching rate does not increase much. The leaching rate of iron increases and then decreases with time. When the roasting time exceeds 2h, the leaching rate of iron decreases significantly. Because calcium exists in the reaction system, when the temperature rises, the Gibbs free energy of the reaction for the formation of calcium sulfate decreases, the energy required for the formation of iron sulfate is greater than the energy required for the formation of calcium sulfate, and sulfuric acid preferentially dissolves calcium. When the reaction time is long, the dissolution of calcium will consume the sulfuric acid required to form iron salts. In other words, the competitive behavior of metal ions affects the production of iron salts and reduces the leaching rate of iron. In addition, when the gypsum obtained by the reaction meets water for a long time, the gypsum will expand and soften, covering the surface of the hematite and hindering its reaction with the acid. Therefore, in order to make the leaching rates of aluminum and iron reach a better level, the roasting time is selected as 2h. The effect of the initial concentration of sulfuric acid on the leaching rate of aluminum and iron is shown in the following figure. Figure 1 c. When the sulfuric acid concentration is low, due to the competition between calcium ions and aluminum ions and iron ions, the chances of aluminum and iron combining with sulfate anions are reduced, resulting in a lower leaching rate of aluminum and iron. As the sulfuric acid concentration increases, the competition continues, but the increase in sulfuric acid reduces this competition, and the aluminum and iron recovery rates therefore increase. When the volume fraction of sulfuric acid is 50%, the leaching rate reaches a peak value. After repeated experiments, the leaching rate can reach up to 99.25% and 99.99%. Figure 1d shows the effect of increasing the volume of sulfuric acid on the leaching rate while keeping the sulfuric acid concentration constant. Increasing the total amount of sulfuric acid will result in an increase in reactants, which is beneficial to many reactions during the red mud roasting process. The water in the reactants will promote the uniform dispersion of the reactants so that all components in the red mud can be reacted thoroughly. However, too much water will cause the gypsum to soften and swell, so the water content should be controlled within the optimal range to facilitate the leaching of aluminum and iron. Obviously, with the increase in the volume of sulfuric acid, the leaching rate of aluminum and iron also increases. When the volume of sulfuric acid is between 10mL and 20mL, the leaching rate of iron increases sharply, and the leaching rate of aluminum also increases significantly, reaching a higher level between 20 and 40mL. In order to ensure a more stable leaching rate, the experiment is based on 40mL of sulfuric acid. This amount of sulfuric acid can save 2.5mL of concentrated sulfuric acid per gram of red mud compared with the previous post-roasting acid leaching process.

[0018] By adjusting the factors affecting water immersion, the water immersion experiment was carried out according to the optimal conditions of the roasting experiment. The conditions of the water immersion experiment were optimized in terms of liquid-to-solid ratio, water immersion time, temperature, and stirring speed. The results are as follows: Figure 2 As shown ( Figure 2 It is composed of four sub-graphs: Figure 2 a. points Figure 2 b. Points Figure 2 c. points Figure 2 d).

[0019] point Figure 2 a describes how the leaching rate of iron increases dramatically with increasing temperature. At the same time, there is no significant effect on the rise in the leaching rate of aluminum. Iron and sulfuric acid react well at relatively high water leaching temperatures. Moreover, at higher temperatures, sulfuric acid molecules dissolved in water are released as gaseous molecules and penetrate the pores of the solid due to the increase in pressure. This causes the solid to break down into finer particles. As a result, the part of the surface that the acid contacts expands, allowing the sulfuric acid reactant to reach the unreacted core. Furthermore, it is known that at high temperatures, the acid molecules are broken down into high-energy active radicals that enter the mineral lattice and can promote the Al 3+ and Fe 3+ Dissolution during water leaching. The effect of liquid-to-solid ratio on leaching rate is mainly reflected in the water content. Water has good fluidity, and the degree of dispersion of reactants immersed in water determines the probability of their mutual collision. The fluidity of water is greater than that of acid. Compared with direct acid leaching, water leaching after roasting can significantly disperse various particles in the reactants, and heating can accelerate the Brownian motion of particles and increase the probability of collision between particles. However, too many water molecules will make the reactant particles too dispersed, thereby reducing the contact probability and reducing the reaction rate. The leaching rate results are shown in the following table. Figure 2b shows that as the liquid-to-solid ratio increases, the leaching first increases and then decreases. When the liquid-to-solid ratio is greater than the most suitable 9 mL / g, the high liquid-to-solid ratio during the leaching process causes the reactants to be over-dispersed and cannot react completely within a certain period of time. When the liquid-to-solid ratio is lower than 9 mL / g, the reactants are a viscous solid-liquid mixture, and the molecular motion is restricted, so that the reaction cannot be completed quickly. The leaching rate results are shown in Figure 2. Figure 2 c shows that with the increase of leaching time, aluminum reaches a higher leaching efficiency at 30min, and there is no obvious change with the increase of time. Because the experimental study is carried out in two stages: sulfuric acid roasting and water leaching separation. During the sulfuric acid roasting process, aluminum preferentially combines with sulfuric acid, so when the aluminum reaction is completed, the iron has not been completely dissolved during the water leaching process. During the roasting process, sulfuric acid reacts with hematite, sulfate ions are adsorbed on the solid surface, and form compounds with iron ions. Finally, water leaching dispersion separates the compounds from the solid surface and releases them better into the solution. The residual sulfuric acid in the reactants needs to be dispersed in a sufficient time to react with the incompletely reacted iron during the water leaching process. However, if the reaction time is too long, sulfuric acid reacts with calcium salts in red mud to produce a large amount of calcium sulfate. Slightly water-soluble calcium sulfate adheres to the surface of red mud particles and has a certain inhibitory effect on the acid leaching reaction. Therefore, when the leaching time is 90min, the leaching rate does not change significantly, while when the leaching time is 120min, the leaching rate decreases significantly. Because the metal activity series is applicable to the reaction of metals with non-oxidizing acids. Aluminum is more active than iron, so sulfuric acid reacts with aluminum first, so the leaching effect of Al is better than that of Fe. When the reaction of aluminum reaches a certain level, iron can be leached in large quantities. The effect of stirring rate on leaching rate is as follows: Figure 2 As shown in Figure d, the leaching rate of aluminum does not change significantly with the increase of stirring speed. This indicates that the leaching reaction of aluminum during water leaching is not significantly affected by the stirring speed. Combined with the influence of leaching time, as the stirring speed increases, the leaching rate of iron also increases. Stirring can accelerate and complete the leaching reaction of iron during water leaching. The reason is that the iron-containing minerals have poor dispersibility during sulfuric acid roasting, and deionized water needs to be added to disperse the iron-containing minerals so that the unreacted internal core can fully react with sulfuric acid. This also explains the necessity of the water leaching process. In addition, the formation of calcium sulfate covers the surface of the iron-containing reactant, and the increase in stirring speed helps to break up the calcium sulfate film on the surface of hematite, allowing sulfuric acid to better contact and react with hematite.

[0020] Scanning electron microscopy was used to examine the morphology of red mud, roasted samples and water-leached residue. Figure 3 As shown ( Figure 3 It is composed of six sub-graphs: Figure 3 a. points Figure 3 b. Points Figure 3 c. points Figure 3 d. points Figure 3 e. points Figure 3 f, where Figure 3 a. points Figure 3 d is the electron microscope image of red mud. Figure 3 b. Points Figure 3 e is the electron microscope image of the calcined sample. Figure 3 c. points Figure 3 f is an electron microscope image of the leached residue).

[0021] point Figure 3 a. points Figure 3 d is the SEM image of the red mud before treatment. It is a state where the columnar structure and the lamellar structure are interwoven and radially embedded. The shape of the columnar structure is uneven. The overall diameter of the red mud in the electron microscope is about 10 mm. The surface of the columnar structure is very dense, making it difficult for the internal material to participate in the chemical reaction. The SEM spectrum of the roasted sample is shown in Figure 2. Figure 3 b. Points Figure 3 e. The dense surface structure breaks down after high temperature roasting with sulfuric acid. The columnar structure of the particles mostly disappears, and the surface is flaky and covered with finer amorphous structures after magnification. The surface becomes more porous and loose, showing obvious signs of erosion. Figure 3 c. points Figure 3 As shown in Figure 5, due to the stirring and soaking during the immersion, the solid surface morphology has changed significantly, and the overall sheet structure has collapsed, and there is no particle column structure in a large area. This morphological change indicates that some mineral phase structures in the red mud have changed. The electron microscope images (i.e., SEM) of roasted red mud with different volumes of sulfuric acid are shown in Figure 5. Figure 4 As shown ( Figure 4 It is composed of six sub-graphs: Figure 4 a. points Figure 4 b. Points Figure 4 c. points Figure 4 d. points Figure 4 e. points Figure 4 f).

[0022] point Figure 4 a. points Figure 4 b. Points Figure 4 c. points Figure 4 d. points Figure 4 e. points Figure 4 f represents the addition of sulfuric acid to red mud at a mass ratio of 0%, 10%, 14%, 16%, 20% and 40%, respectively. As the volume of sulfuric acid increases, the surface structure of red mud changes from particle columnar and flake interlaced to the disappearance of particle columnar, the increase of pores and finally collapse. Figure 6The XRD results of the red mud product show that the surface structure of the red mud collapses to varying degrees. As the volume of sulfuric acid gradually increases, the first thing to react in the red mud structure is the columnar structure of the particles, and small crystals attached to the surface of the lamellar structure are generated. It can be inferred that the columnar structure of the particles may be a mineral with a large amount of aluminum and iron, and the attached structure is the generated solid calcium sulfate. This phenomenon is explained in the unreacted shrinking core, which may be because: the addition of sulfuric acid in the roasting reaction will cause the particles to shrink significantly and the volume of the unreacted core will decrease. When sulfuric acid encounters red mud inside the unreacted core. The easily digestible nature of gibbsite in bauxite forms tiny channels in the red mud particles after the bauxite reacts. At the same time, the pore structure of the red mud is also strengthened. From Figure 5 You can see the SEM of red mud products after sulfuric acid roasting and water leaching of different volumes. Figure 5 c(1), points Figure 5 c(2) shows the surface structure of the leached residue, where most of the iron and aluminum have been leached out. As a result, there are fewer unreacted cores and the overall mineral intensity is finer. Figure 5 f(1), points Figure 5 f(2) can clearly reflect the content of Al and Fe in red mud. The red pixels are the distribution of aluminum, and the green pixels are the distribution of iron. It can be seen that the distribution of aluminum and iron in the original red mud is uniform and abundant. And the distribution of aluminum and iron is not completely consistent. Combined with the XRD results of red mud, it shows that most of the iron may exist alone in hematite. Figure 5 a(1), points Figure 5 a(2), points Figure 5 b(1), points Figure 5 b(2), points Figure 5 c(1), points Figure 5 c(2), points Figure 5 d(1), points Figure 5 d(2), points Figure 5 e(1), points Figure 5 e(2) are the surface morphologies of red mud under different sulfuric acid addition amounts. It can be seen that the surface of red mud is continuously crushed and refined with the increase of sulfuric acid, indicating that the mineral phase in red mud gradually reacts with sulfuric acid.

[0023] The red mud products - raw red mud, roasted samples and water-soaked residues - were subjected to phase analysis. The XRD results are as follows: Figure 6 As shown ( Figure 6 It is divided into Figure 6 (1) Points Figure 6 (2) Composition Figure 6 (1) is a schematic diagram of the phase analysis of the original red mud (c), the roasted sample (b) and the water-soaked residue (a); Figure 6 (2) is a schematic diagram of phase analysis of water-leached slag under different liquid-to-solid ratio conditions).

[0024] Figure 6 Analysis shows that the main minerals containing aluminum and iron in the original red mud include hematite, boehmite, garnet, etc. After hematite is roasted in red mud with high-temperature sulfuric acid, the diffraction peaks of the original mineral phases in the red mud, such as boehmite and calcite, weaken or disappear. New aluminum-iron phases appeared in the roasted samples, among which the chemical formula of Hohmannite with a strong diffraction peak can be written as: Fe3(OH)2(SO4)2·7H2O; at the same time, the impurity peaks in the original red mud ore decreased after roasting. The diffraction peaks of the aluminum-containing ore phase and the iron-containing ore phase in the spectrum of the original red mud ore disappeared in the spectrum of the roasted sample. Complex compounds containing aluminum and iron disappeared in the spectrum of the roasted sample. The diffraction peaks of calcium sulfate (hard gypsum) in the filter residue are obvious and clear, with fewer mixed peaks. The XRD of the activated roasted sample is as follows: Figure 1 (b). Under roasting conditions, the unstable crystal structure of the mineral phase in the red mud first reacts with sulfuric acid. As the sulfuric acid increases, the aluminum and iron elements in the red mud begin to aggregate in the form of soluble sulfates to form compounds. The results show that during the high-temperature sulfuric acid roasting stage, the reaction of the red mud and sulfuric acid mixture at high temperature destroys the difficult-to-break structure in the original red mud ore phase. In the subsequent water leaching process, the newly formed aluminum and iron forms are more likely to enter the solution. The diffraction peaks of the mineral phases of aluminum and iron in the filter residue remaining after leaching are basically weakened or even disappear.

[0025] It is worth noting that vanadium and scandium in red mud mostly exist in the form of isomorphous phases in the crystal lattice of aluminosilicate minerals such as calcium pyroxene. During the sulfuric acid activation and roasting process, the leaching rate of vanadium and scandium reaches more than 98%, which is equivalent to the leaching rate of aluminum in red mud. In addition, when extracting and separating vanadium and scandium, the synergistic extraction of iron ions from metal ions such as aluminum, iron, vanadium, and scandium in the acid leaching solution will have an adverse effect on the extraction and separation of rare and precious metals such as vanadium and scandium. Therefore, the pre-complexation technology is used to stably complex the iron ions in the aqueous phase so that they cannot combine with organic matter during the extraction process, thereby achieving efficient extraction and separation of rare and precious metals such as vanadium. The extraction behavior of Fe(III) in the solution with different amounts of chelating agents EDTA, DTPA, SSA and citric acid was studied, and the color changes of the aqueous phase before and after extraction were recorded. The results are shown in Figure 2. Figure 7 As shown ( Figure 7 It is composed of four sub-graphs: Figure 7 (a), points Figure 7 (b) points Figure 7 (c) points Figure 7 (d) points Figure 7 (a) The complexing agent is EDTA-2Na, Figure 7 (b) The complexing agent is DTPA, Figure 7 (c) The complexing agent is SSA, Figure 7 (d) The complexing agent is citric acid).

[0026] By points Figure 7 (a) shows that with the increase of EDTA-2Na dosage, the extraction rate of Fe(III) decreases rapidly, and its extraction rate reaches the minimum value when the molar ratio of EDTA-2Na:Fe(III) is 1.5, indicating that under this experimental condition, the extractant P507 can hardly extract Fe(III), and then remains relatively constant. It can be concluded that EDTA-2Na has a stronger coordination ability with Fe(III) than P507. In other words, EDTA-2Na forms a more stable complex with Fe(III) in the solution, thereby masking Fe(III) and preventing it from being extracted by the extractant P507. At the same time, EDTA-2Na has extremely low solubility in non-polar organic phase, that is, excess EDTA-2Na will not be dissolved in the organic phase diluted by sulfonated kerosene, and will not affect the recycling of the extractant. Correspondingly, the color change of the aqueous phase before and after extraction is also one-to-one corresponding to the extraction rate. The raffinate (a) is almost colorless, indicating that in the absence of EDTA-2Na, Fe(III) is almost completely extracted into the organic phase by the extractant P507. As the amount of EDTA-2Na continued to increase, the color of the raffinate changed from colorless to light yellow and gradually deepened. When the molar ratio of EDTA-2Na:Fe(III) was greater than 1.5, the color of the solution before and after extraction remained almost unchanged, indicating that EDTA-2Na effectively masked Fe(III) and prevented it from entering the organic phase. Figure 7 The change trend of DTPA in (b) is similar to that of EDTA-2Na. As the molar ratio of DTPA increases from 0 to 1.25, the extraction rate of Fe(Ⅲ) drops sharply until it is less than 1%, and the color of the raffinate gradually darkens until it becomes the color of the original solution. There is no significant change when the dosage of DTPA is increased. This indicates that the chelating ability of the chelating agent DTPA for Fe(Ⅲ) is much greater than the extraction ability of P507 for it. DTPA is also a more suitable chelating agent. At the same time, it can be inferred that the same amount of Fe(Ⅲ) will consume less DTPA. In contrast, the chelating effect of SSA and citric acid is relatively poor. As shown in the figure Figure 7 (c) As the molar ratio of SSA increases from 0 to 2.5, the extraction rate of Fe(Ⅲ) decreases slightly from 85.5% to 54.47%, and maintains a downward trend. This may be due to the fact that the complexing ability of SSA for Fe(Ⅲ) is not as strong as the extraction ability of the extractant P507 for Fe(Ⅲ). From the color comparison before and after extraction, it can be seen that with the increase of the complexing agent, the color of the raffinate deepens to purple, but the color of the raffinate is much lighter than that of the original solution. It can be seen intuitively that SSA has little effect on the extraction of Fe(Ⅲ) by P507. Figure 7(d) Citric acid showed a similar trend: with the increase of citric acid dosage, the extraction rate of Fe(Ⅲ) decreased from 85.5% to 52.21%, and the yellow color of the original solution also turned colorless after extraction. In summary, the addition of EDTA-2Na and DTPA can well affect the extraction effect of extractant P507 on Fe(Ⅲ), so the two complexing agents EDTA-2Na and DTPA were subsequently selected and applied to the vanadium-containing iron simulation solution to explore the optimal experimental conditions.

[0027] After selecting a suitable Fe(Ⅲ) complexing agent, the next step is to study the effect of the addition of the complexing agent on the separation of Fe(Ⅲ) and V(Ⅳ). The effects of the amount of complexing agent DTPA and EDTA-2Na on the separation of solution Fe(Ⅲ) and V(Ⅳ) were studied respectively. The results are as follows Figure 8 As shown ( Figure 8 It is composed of two sub-graphs: Figure 8 (a), points Figure 8 (b) points Figure 8 (a) The complexing agent is DTPA, Figure 8 (b) The complexing agent is EDTA-2Na).

[0028] By points Figure 8 (a) It can be seen that when DTPA is not present, the extraction rate of Fe(III) reaches 96%, and the extraction rate of V(IV) is 94.86%. The results are consistent with the research results of previous researchers [i], that is, the extractant P507 has a good effect on Fe(III) and V(IV), but poor selectivity. As the DTPA molar ratio increases from 0 to 1, the extraction rate of Fe(III) decreases rapidly until it reaches 0, and the extraction rate of V(IV) also decreases slightly. By looking up relevant data to obtain the complexation stability constants of DTPA with different rare earth ions, it can be seen that although the complexation stability constant of V(IV) is much smaller than that of Fe(III), it will inevitably be complexed with DTPA. In particular, as the molar amount of DTPA increases, more DTPA that has not been complexed with Fe(III) will remain to complex with V(IV) in the solution. Therefore, it is particularly important to determine the appropriate molar ratio of DTPA so that it can completely complex Fe(III) without causing the loss of V(IV) due to the complexation with V(IV). By analyzing Figure 8 (b) It can be seen that a 1 molar ratio of DTPA can not only satisfy the complete complexation of Fe(Ⅲ)-DTPA, but also there will be no excess DTPA complexation of V(IV), so a 1 molar ratio of DTPA was selected for subsequent experimental exploration. Figure 8(b) It can be seen that as the EDTA-2Na molar ratio increases from 0 to 1.5, the extraction rate of Fe(Ⅲ) decreases rapidly until it reaches 0, while the extraction rate of V(IV) also decreases slightly. Although the separation of V(IV) and Fe(Ⅲ) can be achieved, the loss of V(IV) will also be caused. At the same time, from the change in the molar ratio of EDTA-2Na and DTPA, it can be seen that less DTPA can achieve the complete complexation of Fe(Ⅲ). Therefore, DTPA was selected as the complexing agent for the separation of vanadium iron solution in subsequent experiments.

[0029] In order to further explore the effect of initial solution pH on vanadium-iron separation, the effect of pH at 0.8-2 and 1 molar ratio of DTPA on vanadium-iron extraction rate was investigated. The results are as follows: Fig. 9 shown.

[0030] Under the premise of maintaining the dosage of DTPA, the extraction rate of Fe(III) does not change much with pH and remains at a level less than 1%. The extraction rate of V(IV) changes significantly with pH, ​​which can be explained by the different existence forms of V(IV) at different pH values ​​mentioned above. As the pH increases from 0.8 to 1.5, the extraction rate of V(IV) shows a continuous upward trend and reaches more than 80%, and further increasing the pH has little effect on it. Therefore, the separation of V(IV) from Fe(III) using the complex separation method should be carried out within the initial pH range of 1.5 to 2.

[0031] DTPA is a pentabasic weak acid. Its complexation reaction process with different ions is very complicated. The complexation order and the form of the complex will also change with experimental conditions such as solution pH, ion concentration and complexation time. By understanding the complexation mechanism, we can choose the appropriate amount of DTPA to make Fe(Ⅲ) complexed more completely and V(IV) not complexed, thereby improving the separation effect and reducing the loss of vanadium. It also effectively reduces the waste of the complexing agent DTPA, thereby minimizing the economic cost. In order to further determine the complexation stoichiometry and complexation form of Fe(Ⅲ) and the complexing agent DTPA, the raffinate after complexation with different molar ratios of DTPA was analyzed by UV-visible spectrophotometry and infrared spectroscopy. Pure distilled water, pure Fe(Ⅲ) solution and raffinate containing different molar ratios of DTPA were measured by UV-visible spectroscopy to obtain the absorbance of different solutions. The results are shown in the following table. Fig.10 shown.

[0032] Depend on Fig.10It can be seen that with the increase in the amount of DTPA used, the peak band between 380-450nm continues to decrease until the molar ratio reaches 1:1, when its value drops to the minimum and remains stable. It is believed that the peak band between 380-450nm is the characteristic peak of Fe(Ⅲ). With the continuous addition of the complexing agent DTPA, Fe(Ⅲ) is continuously complexed and masked to form a DTPA-Fe(Ⅲ) complex, resulting in the continuous weakening of the characteristic peak band. Until the molar ratio is 1:1, Fe(Ⅲ) is completely complexed. The FT-IR spectra of DTPA and DTPA-Fe(Ⅲ) were studied, and the results are as follows: Fig.11 shown.

[0033] Due to the strong hydrogen bonds between molecules, carboxylic acids usually exist in the form of dimers, so DTPA monomers usually exist in the form of dimers in solution. The addition of Fe(III) will depolymerize the dimer form of DTPA to form a more stable complex DTPA-Fe(III). Some features related to the stretching vibration of methylene CH2 were observed at about 3020 cm-1 of DTPA and 1197 cm-1. -1 The peaks on the left and right are considered to be caused by the CN stretching vibration of the functional group. Compared with DTPA, the vibration peak of the carboxylic acid group of DTPA-Fe(Ⅲ) is blue-shifted from 1634.8 cm -1 To 1645.73cm -1 Combined with the results of UV analysis, DTPA and Fe(Ⅲ) complex in a 1:1 form. It is preliminarily believed that the five carboxylic acid groups of DTPA are bonded to Fe(Ⅲ) and a cyclic complex is formed with Fe(Ⅲ) as the center. By comparing DTPA and DTPA-Fe(Ⅲ) complex, the vibration bands of ligand and metal were obtained. Two peaks related to the vibration of iron ligand were found: at 894.88cm -1 The Fe-O vibration peak is located at 455.84 cm -1 These peaks are consistent with the three types of bonds in the preliminarily speculated complex form, so the speculated complex structure is considered to be credible.

[0034] Combining UV-Vis and FT-IR spectroscopy analysis, the structure of the DTPA-Fe(Ⅲ) complex can be inferred. DTPA and Fe(Ⅲ) combine in a 1:1 form, and Fe(Ⅲ) coordinates with five ionized carboxyl oxygen atoms and three nitrogen atoms to form a cyclic complex structure. The specific structure is as follows Fig.12 shown.

[0035] The vanadium and scandium extract residues were used to prepare aluminum-iron composite flocculants. The flocculants prepared under the best preparation conditions were analyzed by infrared spectroscopy to determine the polymerization of starch, aluminum and iron. The results are as follows: Fig.13 shown.

[0036] Depend on Fig.13 The infrared spectra of polyaluminium ferric sulfate (PAFS), modified starch (CTS) and aluminium-iron composite flocculant (PAFS-CTS) are compared, and it can be seen that the material structure of PAFS-CTS has changed compared with PAFS and CTS. -1 ~2919.00cm -1 The absorption peak at 1075cm is the overlapping peak of the stretching vibration of -OH in PSAF, the stretching vibration of OH in CTS, the stretching vibration of CH and the stretching vibration of NH. This broad peak indicates that a large number of intra-chain and inter-chain hydrogen bonds formed by OH and NH are generated in PSAF-CTS. -1 There is an out-of-plane bending vibration absorption peak of -OH at 1143 cm -1 There is also a strong peak at 518cm in PSAF, indicating that -OH in CTS reacts with aluminum or iron to form Al-OH-Al or Fe-OH-Fe, that is, starch reacts with some metal ions. -1 Fe-O vibration at 604 cm -1 The Al-OH vibration disappears at these two absorption peaks, which are consistent with the 610 cm- -1 The OH vibration absorption peak at 612 cm in PAFS-CTS -1 A weak absorption peak appears at

[0037] Fig.14 The scanning electron microscope spectra of aluminum-iron composite flocculants with the total mass ratio of starch to aluminum-iron of 9:1, 5:1, and 1:3 respectively ( Fig.14 It is composed of six sub-graphs: Fig.14 a. points Fig.14 b. Points Fig.14 c. points Fig.14 d. points Fig.14 e. points Fig.14 f composition; Fig.14 a. points Fig.14 The total mass ratio of starch to aluminum and iron in b is 9:1; Fig.14 c. points Fig.14 The total mass ratio of starch to aluminum and iron in d is 5:1; Fig.14 e. points Fig.14 f) The total mass ratio of starch to aluminum and iron is 1:3; the left column is a partial picture, and the right column is the corresponding full picture).

[0038] During the preparation of PSAF-CTS, the modified starch solution is viscous. When it is copolymerized with aluminum sulfate and ferric sulfate solution, the stirring resistance of the solution is large, which hinders the polymerization of aluminum, iron and OH- to form medium and high polymers, which is not conducive to the formation of pore structure. From the above figure, it can be seen that the product presents a scattered block structure when the content of modified starch is less or more, that is, mCTS / m(Al+Fe)=9:1, mCTS / m(Al+Fe)=1:3, and the whole is dispersed small particles, which is not conducive to the flocculation effect; when the modified starch and aluminum iron total mass ratio of the best turbidity reduction effect sample is 5:1, pore structure appears in part of the sample, which is conducive to the coagulation effect of the flocculant.

[0039] The beneficial technical effects of the present invention are as follows: The invention adopts the technology of activated roasting-water leaching, gravity separation, complexation-extraction, graded stripping-precipitation-calcination, and modified starch polymerization of aluminum and iron to comprehensively recover the valuable components of red mud, and obtains various valuable products such as aluminum-iron composite flocculant, vanadium pentoxide, scandium trioxide, anhydrite and white carbon black. The invention has the advantages of many types of valuable component recovery, high recovery rate, high added value of recovered products, no tailings and waste liquid discharge, and broad prospects for comprehensive utilization.

[0040] The technical effects are specifically reflected in: The present invention treats red mud by using the technology of activated roasting-water leaching, gravity separation, complexation-extraction, graded stripping-precipitation-calcination and modified starch polymerization of aluminum and iron to obtain various valuable products such as aluminum-iron composite flocculant, vanadium pentoxide, scandium trioxide, anhydrite and white carbon black. The leaching rate of vanadium is greater than 98%, the leaching rate of scandium is greater than 97%, and the leaching rates of aluminum and iron are greater than 99%. After secondary sorting on a shaking table, the leached residue can obtain anhydrite concentrate with a grade greater than 92% and white carbon concentrate with a grade greater than 95%. The leaching solution uses DTPA to complex iron, and then uses P507 extractant to extract the complexed solution. The vanadium extraction rate is greater than 98%, the scandium extraction rate is greater than 99%, and the aluminum and iron extraction rates are less than 2%, realizing the efficient separation of rare metals vanadium and scandium from aluminum and iron. After secondary stripping, precipitation, and calcination processes, vanadium pentoxide with a purity greater than 99.5% and scandium trioxide with a purity greater than 99.1% can be obtained respectively. The raffinate contains a large amount of aluminum and iron ions. Through the polymerization of modified starch, a high-performance aluminum-iron organic / inorganic composite flocculant can be prepared, wherein the composite flocculant has a total aluminum sulfate iron content greater than 75%. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 Schematic diagram of the influence of various factors on the roasting process ( Figure 1 By by points Figure 1 a. points Figure 1 b. Points Figure 1 c. points Figure 1 d composition).

[0042] Figure 2 Schematic diagram of factors affecting water leaching ( Figure 2 It is divided into Figure 2 a. points Figure 2 b. Points Figure 2 c. points Figure 2 d composition).

[0043] Figure 3 Electron microscope images of red mud, roasted samples, and leached residues ( Figure 3 It is divided into Figure 3 a. points Figure 3 b. Score 0044. Figure 3 c. points Figure 3 d. points Figure 3 e. points Figure 3 f composition; Figure 3 a. points Figure 3 d is the electron microscope image of red mud. Figure 3 b. Points Figure 3 e is the electron microscope image of the calcined sample. Figure 3 c. points Figure 3 f is an electron microscope image of the leached residue).

[0045] Figure 4 is an electron microscope image (i.e., SEM) of roasted red mud with different volumes of sulfuric acid ( Figure 4 It is divided into Figure 4 a. points Figure 4 b. Points Figure 4 c. points Figure 4 d. points Figure 4 e. points Figure 4 f composition; points Figure 4 a. points Figure 4 b. Points Figure 4 c. points Figure 4 d. points Figure 4 e. points Figure 4 f represents the addition of sulfuric acid to the red mud at a mass ratio of 0, 10%, 14%, 16%, 20% and 40%, respectively).

[0046] Figure 5 This is the SEM of red mud products after sulfuric acid roasting and water leaching of different volumes ( Figure 5 It is divided into Figure 5 a(1), points Figure 5 a(2), points Figure 5 b(1), points Figure 5 b(2), points Figure 5 c(1), points Figure 5 c(2), points Figure 5 d(1), points Figure 5 d(2), points Figure 5 e(1), points Figure 5 e(2), points Figure 5 f(1), points Figure 5 f(2) composition; Figure 5 a(1)~point Figure 5 e(2) are the apparent morphologies of red mud under different sulfuric acid addition amounts; Figure 5 f(1), points Figure 5 f(2) can clearly reflect the content of Al and Fe in red mud, where red pixels represent the distribution of aluminum and green pixels represent the distribution of iron).

[0047] Figure 6 This is a schematic diagram of the XRD results of red mud products ( Figure 6 It is divided into Figure 6 (1) Points Figure 6 (2) Composition Figure 6 (1) is a schematic diagram of the phase analysis of the original red mud (c), the roasted sample (b) and the water-soaked residue (a); Figure 6 (2) is a schematic diagram of phase analysis of water-leached slag under different liquid-to-solid ratio conditions).

[0048] Figure 7 Schematic diagram of the effect of different amounts of complexing agents EDTA, DTPA, SSA and citric acid on the extraction behavior of Fe(III) in solution ( Figure 7 It is divided into Figure 7 (a), points Figure 7 (b) points Figure 7 (c) points Figure 7 (d) composition; Figure 7 (a) The complexing agent is EDTA-2Na, Figure 7 (b) The complexing agent is DTPA, Figure 7 (c) The complexing agent is SSA, Figure 7 (d) The complexing agent is citric acid).

[0049] Figure 8 Schematic diagram of the effect of the amount of complexing agent DTPA and EDTA-2Na on the separation of Fe(Ⅲ) and V(Ⅳ) in solution ( Figure 8 It is divided into Figure 8 (a), points Figure 8 (b) Composition Figure 8 (a) The complexing agent is DTPA, Figure 8 (b) The complexing agent is EDTA-2Na).

[0050] Fig. 9 Schematic diagram of the effect of initial solution pH on vanadium-iron separation.

[0051] Fig.10 It is a schematic diagram of the Uv-Vis spectrum of different substances.

[0052] Fig.11 This is a schematic diagram of the infrared spectra of DTPA and DTPA-Fe(Ⅲ) complex.

[0053] Fig.12 It is a schematic diagram of the structure of the DTPA-Fe(III) complex.

[0054] Fig.13 This is the infrared spectrum analysis diagram of the composite flocculant.

[0055] Fig.14 This is a schematic diagram of the SEM spectrum of the composite flocculant ( Fig.14 It is composed of six sub-graphs: Fig.14 a. points Fig.14 b. Points Fig.14 c. points Fig.14 d. points Fig.14 e. points Fig.14 f composition; Fig.14 a. points Fig.14 The total mass ratio of starch to aluminum and iron in b is 9:1; Fig.14 c. points Fig.14 The total mass ratio of starch to aluminum and iron in d is 5:1; Fig.14 e. points Fig.14 f) The total mass ratio of starch to aluminum and iron is 1:3; the left column is a partial picture, and the right column is the corresponding full picture).

[0056] Fig.15 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0057] The present invention will be further described below in conjunction with embodiments (accompanying drawings): To avoid repeated description, the technical parameters involved in the specific implementation of the present invention are uniformly described as follows: the aluminum oxide content in the red mud is 10% to 40%, the iron oxide content is 5 to 20%, the silicon dioxide content is 20 to 40%, the vanadium pentoxide content is 0.05 to 0.6%, and the scandium trioxide content is 0.002 to 0.01%; the leached slag is subjected to gravity separation, and the process is to use a shaking table as a gravity separation equipment, under the separation conditions of a stroke of 8 to 36 mm, a stroke of 240 to 380 times / min, a lateral slope of the bed surface of 0 to 10°, and a separation particle size of 0.01 to 1 mm. After 2-3 levels of shaking table sorting, anhydrite with a grade greater than 92% and white carbon black products with a grade greater than 95% can be obtained; the two-stage stripping, precipitation and calcination process is as follows: first, the loaded organic phase and 2-4 mol / L sulfuric acid solution are mixed at a volume ratio of 10:1-5 and shaken for 5-10 minutes, and static stratification is performed for 3-5 minutes to obtain vanadium-rich liquid and scandium-rich organic phase; then, the scandium-rich organic phase is mixed with 2-4 mol / L sodium hydroxide solution at a volume ratio of 10:1-5 and shaken for 5-10 minutes, and static stratification is performed for 3-5 minutes to obtain a crude scandium hydroxide product and a regenerated organic phase. The vanadium-rich liquid adopts the acidic ammonium salt precipitation method to obtain ammonium polyvanadate (APV) precipitate, and the precipitate is calcined at 450-500°C for 40-60min to obtain vanadium pentoxide (V2O5); the crude scandium hydroxide product is dissolved in sulfuric acid and precipitated with oxalic acid to obtain scandium oxalate precipitate, and the precipitate is washed with water for 3 levels and calcined at 500-600°C for 20-30min to obtain scandium trioxide (Sc2O3); the regenerated organic phase is rinsed with 1-3 mol / L hydrochloric acid solution for 3-5 times and can be continuously used for extraction operation; the modified starch is prepared by etherification chemical modification of corn starch; it will not be repeated in the specific embodiments. Example 1

[0058] During the activation roasting process, the red mud raw material and sulfuric acid are mixed evenly at a mass ratio of 10:1, and then the mixture is placed in an electric furnace with a heating rate of 10°C / min and roasted at a roasting temperature of 200-230°C for 70-90 minutes. After roasting and cooling, the roasted sample is mixed with deionized water at a mass ratio of 1:5, stirred at a leaching temperature of 70-90°C for 60-80 minutes, and after leaching, the leachate and leach residue are obtained by solid-liquid separation. The leachate is pre-complexed, and the process is to adjust the pH value of the leachate to 1.0-1.3 with 1mol / LNaOH and 1mol / LH2SO4, and then add DTPA complexing agent at a solid-liquid mass ratio of 1:10 and stir evenly as the extraction liquid phase, and perform oscillation extraction for 5 minutes at a volume ratio of the extraction liquid phase to the organic phase of 1:1, and perform static stratification for 3 minutes to obtain the raffinate and the loaded organic phase. After two-stage stripping, precipitation and calcination of the loaded organic phase, vanadium pentoxide with a purity greater than 99.8% and scandium trioxide with a purity greater than 99.5% are obtained. The organic phase can be reused after regeneration. The raffinate is polymerized and aged, and the polymerization temperature is set to 30-36°C, and the m (Al+Fe) :m 淀粉 Aluminum sulfate, ferric sulfate and modified starch are added to the raffinate in a ratio of 100:1-4 in sequence, and sodium hydroxide solution is added while stirring to make the pH value 2.5-2.9. After stirring, the mixture is aged for 18-24 hours, and finally spray-dried to obtain an organic / inorganic composite flocculant with a total aluminum sulfate and ferric sulfate content greater than 85%. Example 2

[0059] During the activation roasting process, the red mud raw material and sulfuric acid are mixed evenly at a mass ratio of 10:2, and then the mixture is placed in an electric furnace with a heating rate of 10°C / min and roasted at a roasting temperature of 230-260°C for 50-70 minutes. After roasting and cooling, the roasted sample is mixed with deionized water at a mass ratio of 1:8, stirred at a leaching temperature of 50-70°C for 80-100 minutes, and after leaching, the leachate and leaching residue are obtained by solid-liquid separation. The leachate is pre-complexed, and the process is to adjust the pH value of the leachate to 1.3-1.7 with 1mol / LNaOH and 1mol / LH2SO4, then add DTPA complexing agent at a solid-liquid mass ratio of 2:10 and stir evenly as the extraction liquid phase, and perform oscillation extraction for 7 minutes at a volume ratio of the extraction liquid phase to the organic phase of 2:1, and perform static stratification for 4 minutes to obtain a raffinate and a loaded organic phase. After two-stage stripping, precipitation and calcination of the loaded organic phase, vanadium pentoxide with a purity greater than 99.6% and scandium trioxide with a purity greater than 99.4% are obtained. After the organic phase is regenerated, the raffinate can be reused for polymerization aging operations, and the polymerization temperature is set to 36-43°C, and the m (Al+Fe) :m 淀粉Aluminum sulfate, ferric sulfate and modified starch are added to the raffinate in sequence at a ratio of 100:4-7, and sodium hydroxide solution is added while stirring to make the pH value 2.9-3.2. After stirring, the mixture is aged for 12-18 hours, and finally spray-dried to obtain an organic / inorganic composite flocculant with a total aluminum sulfate and ferric sulfate content greater than 80%. Example 3

[0060] During the activation roasting process, the red mud raw material and sulfuric acid are mixed evenly in a mass ratio of 10:3, and then the mixture is placed in an electric furnace with a heating rate of 10°C / min and roasted at a roasting temperature of 260-300°C for 30-50 minutes. After the roasting is completed and cooled, the roasted sample is mixed with deionized water in a mass ratio of 1:10, stirred for 100-120 minutes at a leaching temperature of 30-50°C, and the leachate and leaching residue are obtained by solid-liquid separation after the leaching is completed. The leachate is pre-complexed, and the process is to adjust the pH value of the leachate to 1.7-2.0 with 1mol / LNaOH and 1mol / LH2SO4, and then add DTPA complexing agent at a solid-liquid mass ratio of 3:10 and stir evenly as the extraction liquid phase, and perform oscillation extraction for 8 minutes at a volume ratio of the extraction liquid phase to the organic phase of 3:1, and perform static stratification for 5 minutes to obtain the raffinate and the loaded organic phase. After two-stage stripping, precipitation and calcination of the loaded organic phase, vanadium pentoxide with a purity greater than 99.5% and scandium trioxide with a purity greater than 99.1% are obtained. The organic phase can be reused after regeneration. The raffinate is polymerized and aged, and the polymerization temperature is set to 43-50°C, and the m (Al+Fe) :m 淀粉 Aluminum sulfate, ferric sulfate and modified starch are added to the raffinate in a ratio of 100:7-10 in sequence, and a sodium hydroxide solution is added while stirring to make the pH value 3.2-3.5. After stirring, the mixture is aged for 6-12 hours, and finally spray-dried to obtain an organic / inorganic composite flocculant with a total aluminum sulfate and ferric sulfate content greater than 75%.

Claims

1. A method for comprehensively recovering multiple valuable components from red mud, characterized in that: The method adopts the technology of activated roasting-water leaching, gravity separation, complexation-extraction, graded stripping-precipitation-calcination, and modified starch polymerization of aluminum and iron to comprehensively recover the valuable components of red mud, and finally obtains aluminum-iron composite flocculant, vanadium pentoxide, scandium trioxide, anhydrite and white carbon black. The specific steps are as follows: a. Red mud activation roasting-water immersion In the activation roasting process, the red mud raw material and sulfuric acid are mixed uniformly in a mass ratio of 10:1-3, and then the mixture is placed in an electric furnace with a heating rate of 10 °C / min, and roasted at a roasting temperature of 200-300 °C for 30-90 minutes; after roasting and cooling, the roasted sample is mixed with deionized water in a mass ratio of 1:5-10, and stirred at a leaching temperature of 30-90 °C for 60-120 minutes. After the leaching is completed, the leachate and the leaching residue are obtained by solid-liquid separation; b. Separation of anhydrite and white carbon black by gravity separation of leaching residue The leached residue obtained in step a is subjected to gravity separation. The specific process is to use a shaking table as a gravity separation device, with a stroke of 8 to 36 mm, a stroke of 240 to 380 times / min, and a transverse slope of 0 to 10 o 2. Under the sorting condition of sorting particle size of 0.01-1 mm, two products, anhydrite and white carbon black, are obtained after 2-3 levels of shaking table sorting; c. Separation and purification of rare and precious metals in the leaching solution The leaching solution obtained in step a is pre-complexed, specifically, the pH value of the leaching solution is adjusted to 1.0-2.0 with 1 mol / L NaOH and 1 mol / L H2SO4, and then DTPA complexing agent is added at a solid-liquid mass ratio of 1-3:10 and stirred evenly as an extraction liquid phase, and the extraction is carried out for 5-8 minutes at a volume ratio of the extraction liquid phase to the organic phase of 1-3:1, and static stratification is carried out for 3-5 minutes to obtain a raffinate and a loaded organic phase; the loaded organic phase is subjected to two-stage stripping, precipitation and calcination to obtain vanadium pentoxide and scandium trioxide, and the organic phase is reused after regeneration; d. Modified polymerization of aluminum / iron in the raffinate The raffinate obtained in step c is subjected to polymerization aging operation, and the polymerization temperature is set to 30-50 o C, according to the mass ratio m (Al+Fe) :m 淀粉 Aluminum sulfate, ferric sulfate and modified starch are added to the raffinate in a ratio of 100:1-10 in sequence, and sodium hydroxide solution is added while stirring to adjust the pH value of the raffinate to 2.5-3.

5. After stirring, the raffinate is aged for 6-24 hours and finally spray-dried to obtain an aluminum-iron composite flocculant.

2. The method for comprehensive recovery of multiple valuable components from red mud according to claim 1, characterized in that: The red mud contains 10% to 40% aluminum oxide, 5% to 20% iron oxide, 20% to 40% silicon dioxide, 0.05% to 0.6% vanadium pentoxide and 0.002% to 0.01% scandium trioxide.

3. The method for comprehensive recovery of multiple valuable components from red mud according to claim 1, characterized in that: The anhydrite and white carbon black are products formed after the red mud is activated and roasted by sulphation. The anhydrite and white carbon black are insoluble in water during the water leaching process and exist in the leached residue. After gravity separation, the grade of anhydrite is greater than 92%, and the grade of white carbon black is greater than 95%.

4. The method for comprehensive recovery of multiple valuable components from red mud according to claim 1, characterized in that: The organic phase is composed of P507 as the main extractant and sulfonated kerosene as the diluent; the process of two-stage stripping, precipitation and calcination: first, the loaded organic phase and 2-4 mol / L sulfuric acid solution are mixed according to a volume ratio of 10:1-5 and shaken for 5-10 minutes, and static stratification is performed for 3-5 minutes to obtain vanadium-rich liquid and scandium-rich organic phase; then, the scandium-rich organic phase is mixed with 2-4 mol / L sodium hydroxide solution according to a volume ratio of 10:1-5 and shaken for 5-10 minutes, and static stratification is performed for 3-5 minutes to obtain a crude scandium hydroxide product and a regenerated organic phase; the vanadium-rich liquid is subjected to an acidic ammonium salt precipitation method to obtain a polyvanadate ammonium precipitate, and the precipitate is calcined at 450-500°C for 40-60 minutes to obtain vanadium pentoxide; the crude scandium hydroxide product is dissolved in sulfuric acid and precipitated with oxalic acid to obtain a scandium oxalate precipitate, and the precipitate is washed with water for 3 stages and then heated at 500-600°C. Calcination at ℃ for 20-30 min to obtain scandium trioxide; The regenerated organic phase is washed 3 to 5 times with 1 to 3 mol / L hydrochloric acid solution and can be continuously used for extraction operations.

5. The method for comprehensive recovery of multiple valuable components from red mud according to claim 1, characterized in that: The purity of the vanadium pentoxide product is greater than 99.5%, and the purity of the scandium trioxide product is greater than 99.1%.

6. The method for comprehensive recovery of multiple valuable components from red mud according to claim 1, characterized in that: The modified starch is prepared by chemically modifying corn starch through etherification.

7. The method for comprehensive recovery of multiple valuable components from red mud according to claim 1, characterized in that: The vanadium concentration in the raffinate is less than 3 ppm, the scandium concentration is less than 0.1 ppm, the aluminum content is greater than 5 g / L, and the iron content is greater than 3 g / L.

8. The method for comprehensive recovery of multiple valuable components from red mud according to claim 1, characterized in that: The total content of aluminum sulfate and iron in the aluminum-iron composite flocculant is greater than 75%, and the flocculant is an organic / inorganic composite material.

Citation Information

Cited By

  • Method for removing ferric oxide in fluorine-containing sludge

    CN120208499A