Aluminum alloy powder for selective laser melting and selective laser melting forming method

By using aluminum alloy powder and atomic atomization method of specific components in laser selection melting technology, a variety of reinforced phases are formed, which solves the problems of thermal cracking and low mechanical properties of aluminum alloy components, and achieves high density and excellent mechanics Properties of aluminum alloy component forming.

CN119061293APending Publication Date: 2024-12-03SHAANXI XINGHUAYE 3D TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310636463.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing laser selection melting technology is prone to thermal cracking tendency and low mechanical properties in forming aluminum alloy components, which affects its application prospects.

Method used

Aluminum alloy powder with specific components, including Fe, Cr, Cu, Mn, Ti, Zr and Si, is prepared by atomic atomization method, controls particle size and loose density, and combines laser selection melting and forming technology to form a variety of Strengthen the phase to improve density and mechanical properties.

Benefits of technology

A crack-free aluminum alloy member is achieved, with a density higher than 99.9%, a tensile strength greater than 400MPa, a yield strength greater than 300MPa, and an elongation greater than 4%, while reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061293A_ABST
    Figure CN119061293A_ABST
Patent Text Reader

Abstract

The invention provides aluminum alloy powder for selective laser melting and a selective laser melting forming method, and belongs to the technical field of laser additive manufacturing. The aluminum alloy powder for selective laser melting, provided by the invention, comprises the following elements in percentage by mass: 1.3 to 1.7 percent of Fe, 1.0 to 1.3 percent of Cr, 0.8 to 1.2 percent of Cu, 0.4 to 0.9 percent of Mn, 0.1 to 0.3 percent of Mg, 0.3 to 0.6 percent of Ti, 0.3 to 0.6 percent of Zr, less than or equal to 0.05 percent of O, less than or equal to 0.1 percent of Si and the balance of Al. Multiple alloy elements are added into an Al matrix, so that multiple strengthening phases can be formed, and the compactness and mechanical property of the aluminum alloy are improved. The density of an aluminum alloy component obtained after selective laser melting forming of the aluminum alloy powder can reach 99.9%, the tensile strength at the room temperature is larger than 400 MPa, the yield strength is larger than 300 MPa, and the ductility is larger than 4%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of laser additive manufacturing, and in particular to an aluminum alloy powder for laser selective melting and a laser selective melting forming method. Background Art

[0002] In recent years, especially in the fields of automobiles, aerospace, etc. where lightweight aluminum alloys are widely used, metal parts with complex morphology and multifunctionality have become an important carrier for realizing the physical integration of multiple components in the modern industrial system. Generally speaking, lightweight aluminum alloys should have excellent mechanical properties and low cost, such as the 2024 aluminum alloy based on the Al-Cu system. However, the processing difficulty of complex parts of 2024 aluminum alloy is large, and the mechanical properties of the formed aluminum alloy parts are poor, which seriously affects its integrated application prospects.

[0003] Selective laser melting (SLM) or laser powder bed fusion (LPBF) can be used to manufacture complex parts. In the research of aluminum alloy systems for laser selective melting, the laser selective melting forming technology of materials such as AlSi12 and AlSi10Mg based on the eutectic Al-Si alloy system is relatively mature, but the mechanical properties of the aluminum alloy components after forming are not high, generally lower than 350MPa; and the traditional medium-strength Al-Cu series and high-strength Al-Zn series aluminum alloys are prone to certain thermal cracking tendencies during the solidification process at the end of laser selective melting due to the large temperature span in the solidification range (such as 2024 or 7075 aluminum alloys), and the rapid cooling and non-equilibrium solidification of additive manufacturing will bring residual tensile stress close to the yield limit, thereby causing cracking of the formed parts.

[0004] Therefore, it is a technical problem that urgently needs to be solved in the art to provide an aluminum alloy powder suitable for laser selective melting forming technology, in which the aluminum alloy components obtained by laser selective melting forming will not crack and can have high mechanical properties. Summary of the invention

[0005] The purpose of the present invention is to provide an aluminum alloy powder for laser selective melting and a method for laser selective melting forming thereof. The aluminum alloy powder for laser selective melting provided by the present invention has no cracking phenomenon, high density and good mechanical properties after laser selective melting forming to obtain an aluminum alloy component.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides an aluminum alloy powder for laser selective melting, comprising the following elements in percentage by mass: Fe 1.3-1.7%, Cr 1.0-1.3%, Cu 0.8-1.2%, Mn 0.4-0.9%, Mg 0.1-0.3%, Ti 0.3-0.6%, Zr 0.3-0.6%, O≤0.05%, Si≤0.1% and the balance Al.

[0008] Preferably, the aluminum alloy powder for selective laser melting comprises the following elements in percentage by mass: Fe 1.35-1.65%, Cr 1.05-1.25%, Cu 0.85-1.15%, Mn 0.45-0.85%, Mg 0.15-0.25%, Ti 0.35-0.55%, Zr 0.35-0.65%, O≤0.04%, Si≤0.08% and the balance Al.

[0009] Preferably, the aluminum alloy powder for selective laser melting further comprises other inevitable impurity elements, and the mass percentage of the other inevitable impurity elements is ≤0.1%.

[0010] Preferably, the particle size distribution of the aluminum alloy powder for selective laser melting is: D10 is 8 to 15 μm, D50 is 20 to 30 μm, and D90 is 35 to 45 μm.

[0011] Preferably, the bulk density of the aluminum alloy powder for laser selective melting is greater than 1.43 g / cm 2 The Hall flow rate of the aluminum alloy powder used for laser selective melting is less than 80s / 50g.

[0012] Preferably, the aluminum alloy powder for selective laser melting is prepared by atomic gas atomization method.

[0013] The present invention also provides a method for selective laser melting, comprising: using a computer to draw a three-dimensional model of the target forming and setting the parameters of selective laser melting, and then using the aluminum alloy powder for selective laser melting described in the above technical solution as a raw material to perform selective laser melting on a substrate to obtain an aluminum alloy component.

[0014] Preferably, the parameters of the laser selective melting forming are: laser power of 340-360W, laser scanning speed of 500-1500mm / s, laser scanning line spacing of 110-130μm, laser scanning interlayer angle of 65-70°, and the thickness of each powder layer is independently 28-32μm.

[0015] Preferably, the preheating temperature of the substrate is 140-170°C.

[0016] Preferably, the aluminum alloy powder for laser selective melting is dried before use; the drying temperature is 110-150° C., the drying time is 2-4 hours; and the drying method is vacuum drying or gas protection drying.

[0017] The present invention provides an aluminum alloy powder for selective laser melting, comprising the following elements in percentage by mass: Fe 1.3-1.7%, Cr 1.0-1.3%, Cu 0.8-1.2%, Mn 0.4-0.9%, Mg 0.1-0.3%, Ti 0.3-0.6%, Zr 0.3-0.6%, O≤0.05%, Si≤0.1% and the balance Al. The aluminum alloy powder for selective laser melting provided by the present invention can form a nano-reinforced phase mainly composed of Al-Fe intermetallic compounds by adding Fe element to the Al matrix; adding Cr element can replace part of the Fe element position to form Al-(Fe, Cr) ternary compounds, such as Al 91 Fe4Cr5 quasicrystals, etc.; adding Cu element can form nano-metallic compounds such as Al2Cu (θ phase); adding Mg element can replace some positions of Cu, thereby obtaining a certain number of Al-Cu-Mg metal compound phases; adding Mn element can replace the Fe element in Al6Fe metal compound to form Al6 (Fe, Mn) phase, thereby optimizing the grain size and morphology of aluminum alloy; adding Ti element can form Al3Ti phase with Al matrix, as a heterogeneous nucleation core, to achieve the transformation of aluminum matrix grains from columnar crystals to equiaxed crystals; adding Zr element can replace Ti element at some positions to obtain Al3 (Ti, Zr) phase, thereby promoting the heterogeneous nucleation effect of aluminum alloy in the process of laser selective melting, which is beneficial to grain refinement and improving tissue density. Therefore, the present invention can form a variety of strengthening phases after adding the above-mentioned multiple alloying elements to Al matrix, thereby effectively improving the density and mechanical properties of aluminum alloy. In addition, the present invention also strictly limits the content of Si and O elements, thereby avoiding the formation of brittle phases and the induction of cracking problems during the laser selective melting process, thereby ensuring that the aluminum alloy component has higher mechanical properties.

[0018] The results of the examples show that the aluminum alloy components obtained by laser selective melting of the aluminum alloy powder provided by the present invention can reach a density of 99.9%, a tensile strength of more than 400 MPa, a yield strength of more than 300 MPa, and an elongation of more than 4% at room temperature. In addition, the aluminum alloy powder provided by the present invention does not add expensive rare earth elements, and has low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a SEM image of the aluminum alloy powder for selective laser melting used in Example 1 of the present invention;

[0020] Figure 2 This is a sample arrangement diagram during the laser selective melting forming process of Examples 1, 4 to 12 of the present invention;

[0021] Figure 3 The density distribution diagram of the aluminum alloy components formed by laser selective melting at different laser scanning speeds in Examples 1, 4 to 12 of the present invention;

[0022] Figure 4 This is a SEM image of the aluminum alloy component sample of Example 1 of the present invention;

[0023] Figure 5 This is a SEM image of the aluminum alloy component sample of Example 5 of the present invention;

[0024] Figure 6 This is a SEM image of the aluminum alloy component sample of Example 9 of the present invention;

[0025] Figure 7 This is a SEM image of the aluminum alloy component sample of Example 12 of the present invention;

[0026] Figure 8 The shape and size diagram of the specimens of the aluminum alloy component specimens of Example 5 and Example 6 of the present invention for tensile testing;

[0027] Fig. 9 It is a tensile test curve diagram of the aluminum alloy component specimens of Example 5 and Example 6 of the present invention. DETAILED DESCRIPTION

[0028] The invention provides an aluminum alloy powder for laser selective melting, comprising the following elements in percentage by mass: Fe 1.3-1.7%, Cr 1.0-1.3%, Cu 0.8-1.2%, Mn 0.4-0.9%, Mg 0.1-0.3%, Ti 0.3-0.6%, Zr 0.3-0.6%, O≤0.05%, Si≤0.1% and the balance Al.

[0029] The aluminum alloy powder for laser selective melting provided by the present invention comprises Fe 1.3-1.7%, preferably 1.35-1.65%, and more preferably 1.4-1.6%, by mass percentage. The present invention can form a nano-reinforced phase mainly composed of Al-Fe intermetallic compounds by adding Fe elements to the Al matrix and controlling the content thereof within the above range, thereby improving the mechanical properties of the aluminum alloy component.

[0030] In terms of mass percentage, the aluminum alloy powder for laser selective melting provided by the present invention includes Cr1.0-1.3%, preferably 1.05-1.25%, and more preferably 1.1-1.2%. By adding Cr element to the Al matrix and controlling its content within the above range, the present invention can replace part of the Fe element position to form Al-(Fe, Cr) ternary compounds, such as Al 91 Fe4Cr5 quasicrystal, etc., thereby effectively enhancing the mechanical properties of aluminum alloy components.

[0031] The aluminum alloy powder for laser selective melting provided by the present invention comprises Cu 0.8-1.2%, preferably 0.85-1.15%, and more preferably 0.9-1.1%, by mass percentage. The present invention forms nano-metallic compounds such as Al2Cu (θ phase) by adding Cu element to the Al matrix and controlling its content within the above range, thereby improving the mechanical properties of the aluminum alloy component as a strengthening phase.

[0032] The aluminum alloy powder for laser selective melting provided by the present invention includes Mn 0.4-0.9%, preferably 0.45-0.85%, and more preferably 0.6-0.8% by mass percentage. By adding Mn element to the Al matrix, the present invention can replace the Fe element in the Al6Fe intermetallic compound to form an Al6(Fe, Mn) phase, thereby optimizing the grain size and morphology of the aluminum alloy, which is more conducive to improving the density and mechanical properties of the aluminum alloy component.

[0033] The aluminum alloy powder for laser selective melting provided by the present invention includes 0.1-0.3% Mg, preferably 0.15-0.25%, and more preferably 0.18-0.22% Mg by mass percentage. The present invention adds Mg element to the Al matrix and controls the content within the above range, so as to replace some positions of Cu, thereby obtaining a certain amount of Al-Cu-Mg intermetallic compound phase, which further serves as a strengthening phase to improve the mechanical properties of the aluminum alloy component.

[0034] The aluminum alloy powder for laser selective melting provided by the present invention includes 0.3-0.6% Ti, preferably 0.35-0.55%, and more preferably 0.4-0.5% Ti by mass percentage. The present invention forms an Al3Ti phase with the Al matrix as a heterogeneous nucleation core by adding the Ti element to the Al matrix and controlling the content thereof within the above range, thereby realizing the transformation of the aluminum matrix grains from columnar crystals to equiaxed crystals, thereby improving the density and mechanical properties of the aluminum alloy component.

[0035] The aluminum alloy powder for laser selective melting provided by the present invention includes Zr0.3-0.6%, preferably 0.35-0.65%, and more preferably 0.4-0.6%, by mass percentage. The present invention adds Zr element to Al matrix and controls its content within the above range. Zr element can be substituted with Ti element at some positions to obtain Al3 (Ti, Zr) phase, thereby promoting its heterogeneous nucleation, facilitating grain refinement, improving tissue density and mechanical properties.

[0036] In terms of mass percentage, the aluminum alloy powder for laser selective melting provided by the present invention includes O≤0.05%, preferably ≤0.04%, and more preferably ≤0.03%. By controlling the O content within the above range, the present invention can avoid the formation of brittle phases and the induction of cracking during the laser selective melting process, thereby ensuring that the aluminum alloy component has higher mechanical properties.

[0037] In terms of mass percentage, the aluminum alloy powder for laser selective melting provided by the present invention includes Si≤0.1%, preferably≤0.08%, and more preferably≤0.07%. By controlling the Si content within the above range, the present invention can avoid the formation of brittle phases and the induction of cracking during the laser selective melting process, thereby ensuring that the aluminum alloy component has higher mechanical properties.

[0038] Measured by mass percentage, the aluminum alloy powder for selective laser melting provided by the present invention includes a remainder of Al.

[0039] The aluminum alloy powder for laser selective melting provided by the present invention also includes other inevitable impurity elements, and the mass percentage of the other inevitable impurity elements is ≤0.1%. By limiting the content of other impurity elements, the present invention can reduce the influence of other impurity elements on the structure of aluminum alloy components as much as possible, and ensure that the aluminum alloy components have higher mechanical properties.

[0040] In the present invention, the particle size distribution of the aluminum alloy powder for laser selective melting is preferably: D10 is 8-15 μm, D50 is 20-30 μm, and D90 is 35-45 μm. The particle size distribution of the aluminum alloy powder for laser selective melting in the present invention is within the above range, so that the powder particles can be more closely contacted and have better fluidity, which is more conducive to obtaining a high-density aluminum alloy component by laser selective melting of the aluminum alloy powder.

[0041] In the present invention, the bulk density of the aluminum alloy powder for laser selective melting is preferably greater than 1.43 g / cm 2 , more preferably 1.43 to 2.5 g / cm 2The Hall flow rate of the aluminum alloy powder for laser selective melting is preferably less than 80s / 50g, and more preferably 50s / 50g to 80s / 50g. The present invention controls the bulk density and Hall flow rate of the aluminum alloy powder for laser selective melting within the above range, which is more conducive to the aluminum alloy component to obtain higher density and mechanical properties.

[0042] In the present invention, the aluminum alloy powder for laser selective melting is preferably prepared by atomic gas atomization. The present invention has no special requirements on the process conditions of the atomic gas atomization method, and the preparation can be carried out by the conventional atomic gas atomization method in the art. The present invention prepares the aluminum alloy powder for laser selective melting by atomic gas atomization, so that the aluminum alloy powder has a higher sphericity, reduces the internal defects of the spherical particles, and is more conducive to obtaining aluminum alloy components with high density and excellent mechanical properties.

[0043] The aluminum alloy powder for selective laser melting provided by the present invention has no cracking phenomenon, high density and good mechanical properties after laser selective melting and forming, and the aluminum alloy powder for selective laser melting provided by the present invention has no expensive rare earth elements added and has low cost.

[0044] The present invention also provides a method for selective laser melting, comprising: using a computer to draw a three-dimensional model of the target forming and setting the parameters of selective laser melting, and then using the aluminum alloy powder for selective laser melting described in the above technical solution as a raw material to perform selective laser melting on a substrate to obtain an aluminum alloy component.

[0045] In the present invention, the parameters of the laser selective melting forming are preferably: laser power of 340-360W, laser scanning speed of 500-1500mm / s, laser scanning line spacing of 110-130μm, laser scanning layer angle of 65-70°, and the thickness of each powder layer is independently 28-32μm; more preferably: laser power of 350W, laser scanning speed of 600-1200mm / s, laser scanning line spacing of 120μm, laser scanning layer angle of 67°, and the thickness of each powder layer is independently 30μm.

[0046] In the present invention, the preheating temperature of the substrate is preferably 140-170° C., more preferably 150-170° C. By controlling the preheating temperature of the substrate within the above range, the present invention can reduce the temperature difference between the first layer of aluminum alloy powder that has been melted during laser selective melting and the substrate, thereby avoiding problems such as cracks induced by rapid cooling.

[0047] The present invention has no special requirements on the material of the substrate, and a conventional substrate used for laser selective melting forming in the art can be used.

[0048] In the present invention, the aluminum alloy powder for laser selective melting is preferably dried before use; the drying temperature is preferably 110-150°C, more preferably 120°C; the drying time is preferably 2-4h, more preferably 2.5-3.5h; the drying method is preferably vacuum drying or gas-protected drying.

[0049] The laser selective melting forming method provided by the present invention can better shape aluminum alloy powder, avoid cracking and other problems in the prepared aluminum alloy components, and ensure that the prepared aluminum alloy components have higher density and mechanical properties.

[0050] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0051] Example 1

[0052] The aluminum alloy powder for selective laser melting in this embodiment is composed of the following elements in percentage by mass: Fe 1.5%, Cr 1.2%, Cu 1%, Mn 0.6%, Mg 0.2%, Ti 0.45%, Zr 0.45%, O 0.01%, Si 0.04% and the balance Al and other inevitable impurity elements ≤0.1%.

[0053] The particle size distribution of the aluminum alloy powder for laser selective melting is as follows: D10 is 9 to 14 μm, D50 is 22 to 28 μm, and D90 is 35 to 43 μm.

[0054] The bulk density of the aluminum alloy powder for laser selective melting is 1.46 g / cm 2 The Hall flow rate of the aluminum alloy powder used for laser selective melting is 75s / 50g.

[0055] The aluminum alloy powder for laser selective melting is prepared by atomic gas atomization method.

[0056] The method for laser selective melting forming using the above-mentioned aluminum alloy powder for laser selective melting as raw material is as follows: using a computer to draw a three-dimensional model of the target forming and set the parameters of laser selective melting, and then laser selective melting the vacuum dried aluminum alloy powder raw material for laser selective melting on a substrate to obtain an aluminum alloy component. Wherein, the preheating temperature of the substrate is 150°C, the vacuum drying temperature of the aluminum alloy powder raw material for laser selective melting is 120°C, and the vacuum drying time is 2.5h; the parameters of laser selective melting are: laser power is 350W, laser scanning speed is 700mm / s, laser scanning line spacing is 120μm, laser scanning layer angle is 67°, and the thickness of each powder layer is 30μm.

[0057] Example 2

[0058] The aluminum alloy powder for laser selective melting in this embodiment is composed of the following elements in mass percentage: Fe 1.6%, Cr 1.3%, Cu 1.2%, Mn 0.8%, Mg 0.3%, Ti 0.6%, Zr 0.6%, O 0.03%, Si 0.05% and the balance Al and other unavoidable impurity elements ≤ 0.1%. The remaining technical features are the same as those in Example 1.

[0059] Example 3

[0060] The aluminum alloy powder for laser selective melting in this embodiment is composed of the following elements in mass percentage: Fe 1.3%, Cr 1%, Cu 0.8%, Mn 0.5%, Mg 0.1%, Ti 0.3%, Zr 0.3%, O 0.01%, Si 0.01% and the balance Al and other unavoidable impurity elements ≤0.1%. The remaining technical features are the same as those in Example 1.

[0061] Embodiments 4 to 12

[0062] The laser scanning speed in the laser selective melting parameters in Example 1 was replaced by 600mm / s, 800mm / s, 900mm / s, 1000mm / s, 1100mm / s, 1200mm / s, 1300mm / s, 1400mm / s and 1500mm / s, respectively, and they were respectively used as Examples 4 to 12, and the remaining technical features were the same as those in Example 1. The aluminum alloy components of Examples 1 to 3 were subjected to density detection based on image analysis, using the software Image J, and the photos from different regions and different cross-sectional positions were counted three times. The density results of the samples obtained by the detection are shown in Table 1. The aluminum alloy component samples of Examples 1 to 3 were subjected to room temperature tensile tests at a tensile rate of 1mm / min according to the national standard GB / T228.1, and the mechanical properties were tested. The test results are shown in Table 1.

[0063] Table 1 Density and room temperature mechanical properties test results of aluminum alloy component samples of Examples 1 to 3

[0064] Example 1 Example 2 Example 3 Density / % 99.9 99.8 99.9 Tensile strength / MPa 391 425 365 Yield strength / MPa 313 341 302 Elongation / % 3.3 3.2 5.2

[0065] It can be seen from Table 1 that the density of the aluminum alloy component samples of Examples 1 to 3 can reach 99.8 to 99.9%, the tensile strength can reach 365 to 425 MPa, the yield strength can reach 302 to 341 MPa, and the elongation can reach 3.2 to 5.2%. It can be seen that the aluminum alloy powder for laser selective melting provided by the present invention can enable the aluminum alloy component to obtain a higher density and excellent mechanical properties when used for laser selective melting forming to prepare the aluminum alloy component.

[0066] The aluminum alloy powder for laser selective melting used in Example 1 was observed for its microscopic morphology using a scanning electron microscope. The SEM image obtained by observation is as follows: Figure 1 shown.

[0067] Depend on Figure 1 It can be seen that the aluminum alloy powder used for laser selective melting is a dispersed and uniform spherical powder, and its particle size is distributed within a certain range. The small-particle spherical powder can fill the pores between the large-particle powder, which is more conducive to improving the density of the aluminum alloy components.

[0068] The sample distribution during laser selective melting in Examples 1, 4 to 12 is shown in Figure 2 , where each sample size is 8×8×8mm 3 .Depend on Figure 2 It can be seen that in order to ensure the repeatability of the experiment, two forming experiments at different positions were carried out for each process parameter.

[0069] The aluminum alloy components obtained by laser selective melting in Examples 1, 4 to 12 were subjected to density detection based on image analysis. The software Image J was used to count photos from different regions and cross-sectional positions three times. The density results of the samples obtained by the detection were as follows: Figure 3 As shown, Figure 3 The corresponding specific density values ​​are shown in Table 2.

[0070] Table 2 Density test results of aluminum alloy components obtained by laser selective melting forming in Examples 1, 4 to 12

[0071] Laser scanning speed (mm / s) Density(%) Example 4 600 99.1 Example 1 700 99.9 Example 5 800 99.9 Example 6 900 99.9 Example 7 1000 99.8 Example 8 1100 99.7 Example 9 1200 97.8 Example 10 1300 97.3 Embodiment 11 1400 95.9 Example 12 1500 94.5

[0072] Depend on Figure 3It can be seen from Table 2 that when the laser scanning speed is in the range of 600-1100 mm / s, the density of the aluminum alloy component can reach more than 99%. Continuing to increase the laser scanning speed will reduce the density of the aluminum alloy component. This may be because the laser scanning speed increases, the input energy density decreases, and the molten pool of ideal size cannot be formed, and then unfused defects will appear between the molten pools, reducing the density.

[0073] The microstructures of the aluminum alloy components prepared in Example 1, Example 5, Example 9, and Example 12 at laser scanning speeds of 700 mm / s, 800 mm / s, 1200 mm / s, and 1500 mm / s were observed by scanning electron microscopy. The results are as follows: Figures 4 to 7 As shown; among them, Figure 4 This is the SEM image of the aluminum alloy component sample of Example 1. Figure 5 This is the SEM image of the aluminum alloy component sample of Example 5. Figure 6 This is the SEM image of the aluminum alloy component sample of Example 9. Figure 7 This is the SEM image of the aluminum alloy component sample of Example 12.

[0074] Depend on Figures 4 to 7 It can be seen that when the laser scanning speed is 700 mm / s, the density of the sample is the highest and no obvious metallurgical defects are observed. Similarly, when the laser scanning speed is slightly increased to 800 mm / s, the metallurgical defects remain at a relatively low level. When the scanning speed is further increased to 1200 mm / s, the defect content increases significantly, first of all, small-sized spherical defects. At a laser scanning speed of 1500 mm / s, there are a large number of unfused defects inside the sample, and their morphology is irregular.

[0075] In order to maximize production efficiency, the scanning speed should be maintained at a high level. Therefore, the aluminum alloy component samples of Example 5 and Example 6 were subjected to room temperature tensile tests to test their mechanical properties at a tensile rate of 1 mm / min according to the national standard GB / T228.1. The shape and size of the sample used in the tensile test are as follows: Figure 8 The tensile test results are shown in Fig. 9 As shown (wherein Example 5 refers to Embodiment 5, and Example 6 refers to Embodiment 6).

[0076] Depend on Fig. 9 It can be seen that the aluminum alloy component obtained by laser selective melting of the aluminum alloy powder provided by the present invention has a tensile strength greater than 400 MPa, a yield strength greater than 300 MPa, and an elongation greater than 4% at room temperature.

[0077] It can be seen from the above embodiments that the aluminum alloy powder for laser selective melting provided by the present invention has high density, no cracking problem and good mechanical properties after laser selective melting to obtain the aluminum alloy component.

[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. An aluminum alloy powder for selective laser melting, characterized in that: The invention comprises the following elements in percentage by mass: Fe 1.3-1.7%, Cr 1.0-1.3%, Cu 0.8-1.2%, Mn 0.4-0.9%, Mg 0.1-0.3%, Ti 0.3-0.6%, Zr 0.3-0.6%, O≤0.05%, Si≤0.1% and the balance Al.

2. The aluminum alloy powder for selective laser melting according to claim 1, characterized in that: The invention comprises the following elements in percentage by mass: Fe 1.35-1.65%, Cr 1.05-1.25%, Cu 0.85-1.15%, Mn 0.45-0.85%, Mg 0.15-0.25%, Ti 0.35-0.55%, Zr 0.35-0.65%, O≤0.04%, Si≤0.08% and the balance Al.

3. The aluminum alloy powder for selective laser melting according to claim 1 or 2, characterized in that: The aluminum alloy powder for selective laser melting also includes other inevitable impurity elements, and the mass percentage of the other inevitable impurity elements is ≤0.1%.

4. The aluminum alloy powder for selective laser melting according to claim 1 or 2, characterized in that: The particle size distribution of the aluminum alloy powder for laser selective melting is as follows: D10 is 8 to 15 μm, D50 is 20 to 30 μm, and D90 is 35 to 45 μm.

5. The aluminum alloy powder for selective laser melting according to claim 1 or 2, characterized in that: The bulk density of the aluminum alloy powder for laser selective melting is greater than 1.43 g / cm 2 The Hall flow rate of the aluminum alloy powder used for laser selective melting is less than 80s / 50g.

6. The aluminum alloy powder for selective laser melting according to claim 1 or 2, characterized in that: The aluminum alloy powder for laser selective melting is prepared by atomic gas atomization method.

7. A method for selective laser melting, characterized in that: include: A computer is used to draw a three-dimensional model of the target forming and set the parameters of laser selective melting, and then the aluminum alloy powder for laser selective melting according to any one of claims 1 to 6 is used as a raw material to perform laser selective melting on a substrate to obtain an aluminum alloy component.

8. The method for selective laser melting as claimed in claim 7, characterized in that: The parameters of the laser selective melting forming are: laser power of 340-360W, laser scanning speed of 500-1500mm / s, laser scanning line spacing of 110-130μm, laser scanning layer angle of 65-70°, and the thickness of each powder layer is independently 28-32μm.

9. The method for selective laser melting as claimed in claim 7, characterized in that: The preheating temperature of the substrate is 140-170°C.

10. The method for selective laser melting as claimed in claim 7, characterized in that: The aluminum alloy powder for laser selective melting is dried before use; the drying temperature is 110-150° C., the drying time is 2-4 hours; and the drying method is vacuum drying or gas protection drying.