Preparation process of nano aluminum alloy material for electric power fittings
By adding specific elements and processes to the aluminum alloy, the problem of insufficient strength of copper-aluminum electric power tools is solved, high strength, corrosion resistance and lightweight are achieved, and the service life of the tools is extended.
Patent Information
- Application Number
- CN202411569875.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-06
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing copper-aluminum electric power tools are broken due to insufficient strength during use, which increases maintenance costs and is highly risky, and it is difficult to achieve lightweight and high reliability.
Using nano-aluminum alloy materials, the nano-extracted nano-extracted nano-extracted nano-extracted nano-extracted nano-extracted nano-extracted nano-extracted nano-extracted nano-extracted products are added to the aluminum alloy by adding silicon, boron, platinum, cadmium, primula, primula, primula, and primophylla to the aluminum alloy. Aluminum alloy materials are used in electrical appliances.
It significantly improves the mechanical properties and wear resistance of aluminum alloys, extends the service life of electric power tools, and is suitable for complex environments, reducing maintenance costs.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloys and preparation thereof, and in particular, relates to a preparation process of a nano aluminum alloy material for electric power fittings. Background Art
[0002] Power fittings are mainly divided into several categories according to materials, such as copper and aluminum, steel, and ferrous metal. Among them, copper and aluminum are the main category. With the increasing use of power fittings and the increase in usage, higher requirements are placed on the lightweight, corrosion-resistant, and high-strength characteristics of power fittings. At present, after a certain number of uses, copper and aluminum power fittings will break due to insufficient strength, which not only increases maintenance costs, but also has a high risk factor. Therefore, achieving lightweight fittings and ensuring high reliability in service is still a requirement for current technical development. Summary of the invention
[0003] The primary purpose of the present invention is to provide a nano aluminum alloy material for electric power fittings and its preparation process, so as to achieve lightweight, corrosion resistance and high strength of aluminum alloy, and to achieve lightweight of electric power fittings and extend the service life of electric power fittings.
[0004] To this end, the present invention provides the following technical solutions.
[0005] One aspect of the present invention provides a nano aluminum alloy material for electric power fittings, characterized in that, measured by mass percentage, the nano aluminum alloy material contains the following constituent raw materials: 1.25-7.25% tungsten, 0.75-3% silicon, 0.01-0.05% boron, 1-5% copper, 0.5-1% platinum, 2.15-6.75% cadmium, 0.5-1% nickel, 0.05-0.25% lutetium, 0.03-0.2% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0006] In a preferred embodiment of the present invention, the nano aluminum alloy material contains the following raw materials in percentage by mass: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0007] Another aspect of the present invention also provides a method for preparing a nano aluminum alloy material for electric power fittings, the method comprising the following steps: S1: Under an inert atmosphere, each raw material is ball-milled in turn, and then passed through a 2000-5000 mesh sieve to obtain each raw material powder; S2: mixing the obtained raw material powders and adding a dispersant to fully stir to obtain a mixture; S3: subjecting the obtained mixture to compression molding to obtain a green body; S4: sintering the obtained green body at high temperature, keeping the temperature and then cooling to room temperature to obtain a nano aluminum alloy material.
[0008] In a preferred embodiment of the present invention, in step S1, the ball milling conditions are: ball-to-material ratio of 10-15:1, rotation speed of 400-800 rpm, and time of 12-24 hours.
[0009] In a preferred embodiment of the present invention, in step S1, the ball milling is wet ball milling, and the solvent of the wet ball milling is selected from any one of water, ethanol and kerosene.
[0010] In a preferred embodiment of the present invention, in step S1, the inert atmosphere is selected from any one of argon, nitrogen and helium.
[0011] In a preferred embodiment of the present invention, in step S2, the dispersant is selected from any one of vinyltriethoxysilane, vinyltrimethoxysilane and vinyltri(β-methoxyethoxy)silane.
[0012] In a preferred embodiment of the present invention, the amount of the dispersant added is 0.03 to 0.1 times the total amount of the raw materials.
[0013] In a preferred embodiment of the present invention, in step S3, the molding treatment conditions are: pressure 800-1200 MPa, time 1-3 min.
[0014] In a preferred embodiment of the present invention, in step S4, the high temperature sintering conditions are: temperature 1000-2000° C., time 4-8 hours.
[0015] Another aspect of the present invention provides a use of the nano aluminum alloy material as described above in the preparation of electric power fittings.
[0016] By means of the above technical solution, the present invention has at least the following advantages: The present invention adds two non-metals, silicon and boron, to the aluminum alloy, and simultaneously adds platinum and cadmium metals, as well as lutetium and praseodymium rare earth metals. Through the synergistic effect between the three types of elements, the present invention has an obvious strengthening effect, so that the mechanical strength and corrosion resistance of the obtained aluminum alloy are improved. When used in the application of electric power fittings, the mechanical properties of the product can be improved and the service life of the product can be extended.
[0017] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION
[0018] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] Unless otherwise specified, the percentage content involved in the present invention refers to mass percentage for solid-liquid mixing and solid-solid mixing, and refers to volume percentage for liquid-liquid mixing.
[0020] Unless otherwise specified, the percentage concentrations referred to in the present invention all refer to final concentrations, which refer to the percentage of the added component in the system after the addition of the component.
[0021] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.
[0022] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods.
[0023] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources. Example
[0024] In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0025] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material. Example
[0026] In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 7.25% tungsten, 0.75% silicon, 0.05% boron, 1% copper, 1% platinum, 2.15% cadmium, 1% nickel, 0.05% lutetium, 0.2% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0027] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: ethanol) at a ball-to-material ratio of 15:1 for 24 h at 400 rpm, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyltrimethoxysilane (the added amount is 0.1 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 800 MPa for 3 min to obtain a green body; S4: The obtained green body is sintered at 1000° C. for 8 h, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material. Example
[0028] In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 1.25% tungsten, 3% silicon, 0.01% boron, 5% copper, 0.5% platinum, 6.75% cadmium, 0.5% nickel, 0.25% lutetium, 0.03% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0029] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (the solvent was kerosene) at a ball-to-material ratio of 10:1 for 12 h at 800 rpm, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl tri(β-methoxyethoxy)silane (the added amount is 0.03 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1200 MPa for 1 min to obtain a green body; S4: The obtained green body is sintered at 2000° C. for 4 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material. Example
[0030] In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 2.25% tungsten, 1.5% silicon, 0.04% boron, 2% copper, 0.9% platinum, 3.75% cadmium, 0.6% nickel, 0.1% lutetium, 0.1% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0031] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 12:1 at a speed of 500 rpm for 22 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.05 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 900 MPa for 2.5 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material. Example
[0032] In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 6.25% tungsten, 2.5% silicon, 0.02% boron, 4% copper, 0.6% platinum, 5.75% cadmium, 0.9% nickel, 0.2% lutetium, 0.2% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0033] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: ethanol) at a ball-to-material ratio of 13:1 at a speed of 700 rpm for 20 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyltrimethoxysilane (the added amount is 0.08 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1100 MPa for 1.5 min to obtain a green body; S4: The obtained green body is sintered at 1000° C. for 8 h, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0034] Comparative Example 1: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 4.25% tungsten, 0.03% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0035] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0036] Comparative Example 2: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 4.25% tungsten, 1.875% silicon, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0037] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0038] Comparative Example 3: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 4.25% tungsten, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0039] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0040] Comparative Example 4: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0041] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0042] Comparative Example 5: In this embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material contains the following raw materials in terms of mass percentage: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% platinum, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0043] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0044] Comparative Example 6: In this embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material contains the following raw materials in terms of mass percentage: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0045] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0046] Comparative Example 7: In this embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material contains the following raw materials in terms of mass percentage: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0047] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0048] Comparative Example 8: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0049] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0050] Comparative Example 9: In this embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material contains the following raw materials in terms of mass percentage: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0051] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0052] Comparative Example 10: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 0.25% tungsten, 0.2% silicon, 0.06% boron, 6% copper, 0.15% platinum, 1% cadmium, 0.3% nickel, 0.35% lutetium, 0.3% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0053] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0054] Comparative Example 11: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 0.25% tungsten, 4% silicon, 0.08% boron, 0.5% copper, 1.5% platinum, 7% cadmium, 2% nickel, 0.6% lutetium, 0.01% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0055] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0056] Comparative Example 12: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 8% tungsten, 0.5% silicon, 0.06% boron, 6% copper, 2% platinum, 1% cadmium, 0.1% nickel, 0.01% lutetium, 0.3% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0057] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0058] Comparative Example 13: In the present embodiment, a nano-aluminum alloy material for electric power fittings is provided. The nano-aluminum alloy material comprises the following constituent raw materials in percentage by mass: 4.25% tungsten, 0.2% silicon, 0.06% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.01% lutetium, 0.3% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
[0059] A method for preparing a nano aluminum alloy material for electric power fittings comprises the following steps: S1: Under argon atmosphere, the raw materials were wet-milled (solvent: water) at a ball-to-material ratio of 10:1 at a speed of 600 rpm for 18 h, and then passed through a 2000 mesh sieve to obtain raw material powders; S2: Mix the obtained raw material powders and add vinyl triethoxysilane (the added amount is 0.065 times the total amount of the raw materials) and stir well to obtain a mixture; S3: The obtained mixture is subjected to compression molding at 1000 MPa for 2 min to obtain a green body; S4: The obtained green body is sintered at 1500° C. for 6 hours, kept warm and then cooled to room temperature to obtain a nano aluminum alloy material.
[0060] Test 1: Mechanical properties of different alloys Experimental objects: Examples 1-5 and Comparative Examples 1-13, alloy sizes are all 50 mm × 100 mm; Experimental methods: 1) Corrosion resistance test is carried out with reference to GB / T 7998-2005.
[0061] 2) The conditions of the friction and wear test are: a friction and wear disk of No. 45 hardened steel, a load of 200N, a friction linear speed of 0.5m / s, a test time of 30min, a relative humidity of 35% in the test environment, and an ambient temperature of 25%.
[0062] The results are shown in Table 1.
[0063] Table 1 Mechanical properties and corrosion resistance of different alloys Group Tensile strength (MPa) Yield strength (MPa) Corrosion level Friction and wear loss weight (mg) Example 1 498 437 1 0.22 Example 2 502 443 1 0.23 Example 3 489 426 1 0.27 Example 4 493 441 1 0.25 Example 5 491 434 1 0.28 Comparative Example 1 468 402 1 0.32 Comparative Example 2 470 412 1 0.29 Comparative Example 3 459 406 1 0.34 Comparative Example 4 452 401 2 0.37 Comparative Example 5 431 373 2 0.41 Comparative Example 6 413 357 3 0.50 Comparative Example 7 465 395 2 0.33 Comparative Example 8 459 389 2 0.35 Comparative Example 9 441 375 3 0.39 Comparative Example 10 481 409 1 0.28 Comparative Example 11 482 421 1 0.29 Comparative Example 12 475 413 1 0.28 Comparative Example 13 471 409 2 0.30 It can be seen from the results in Table 1 that, compared with comparative examples 1-13, the aluminum alloys prepared in Examples 1-5 of the present invention have the advantages of high strength, good wear resistance and good corrosion resistance. The aluminum alloys of the present invention can be used in electric power fittings products, which can be applied to more complex climates and working environments, improve the performance of electric power fittings, and extend the service life of the fittings.
[0064] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A nano aluminum alloy material for electric power fittings, characterized in that: The nano-aluminum alloy material contains the following raw materials in terms of mass percentage: 1.25-7.25% tungsten, 0.75-3% silicon, 0.01-0.05% boron, 1-5% copper, 0.5-1% platinum, 2.15-6.75% cadmium, 0.5-1% nickel, 0.05-0.25% lutetium, 0.03-0.2% praseodymium, and the remainder of aluminum and other unavoidable impurities, and the impurity content is not higher than 0.01%.
2. The nano aluminum alloy material for electric power fittings according to claim 1, characterized in that: Measured by mass percentage, the nano-aluminum alloy material contains the following constituent raw materials: 4.25% tungsten, 1.875% silicon, 0.03% boron, 3% copper, 0.75% platinum, 4.45% cadmium, 0.75% nickel, 0.15% lutetium, 0.115% praseodymium, and the remainder of aluminum and other inevitable impurities, and the impurity content is not higher than 0.01%.
3. The method for preparing a nano-aluminum alloy material for electric power fittings according to claim 1 or 2, characterized in that: The method comprises the following steps: S1: Under an inert atmosphere, each raw material is ball-milled in sequence, and then passed through a 2000-5000 mesh sieve to obtain each raw material powder; S2: mixing the obtained raw material powders and adding a dispersant and stirring thoroughly to obtain a mixture; S3: molding the obtained mixture to obtain a green body; S4: sintering the obtained green body at high temperature, keeping the temperature and then cooling to room temperature to obtain a nano aluminum alloy material.
4. The method for preparing nano aluminum alloy material for electric power fittings according to claim 3, characterized in that: In step S1, the ball milling conditions are: ball-to-material ratio of 10-15:1, rotation speed of 400-800 rpm, and time of 12-24 h.
5. The method for preparing nano aluminum alloy material for electric power fittings according to claim 3, characterized in that: In step S1, the ball milling is wet ball milling, and the solvent of the wet ball milling is selected from any one of water, ethanol, and kerosene.
6. The method for preparing nano aluminum alloy material for electric power fittings according to claim 3, characterized in that: In step S1, the inert atmosphere is selected from any one of argon, nitrogen, and helium.
7. The method for preparing nano aluminum alloy material for electric power fittings according to claim 3, characterized in that: In step S2, the dispersant is selected from any one of vinyltriethoxysilane, vinyltrimethoxysilane, and vinyltri(β-methoxyethoxy)silane; and the amount of the dispersant added is 0.03 to 0.1 times the total amount of the raw materials.
8. The method for preparing nano aluminum alloy material for electric power fittings according to claim 3, characterized in that: In step S3, the molding treatment conditions are: pressure 800-1200 MPa, time 1-3 min.
9. The method for preparing nano aluminum alloy material for electric power fittings according to claim 3, characterized in that: In step S4, the high temperature sintering conditions are: temperature 1000-2000° C., time 4-8 hours.
10. Use of the nano aluminum alloy material according to claim 1 or 2 in the preparation of electric power fittings.
Citation Information
Patent Citations
W-RE high-strength heat-resisting aluminium alloy material and preparation method thereof
CN101805851A
Ni-W-RE high-strength heat-resistant aluminium alloy material and preparation method thereof
CN101994042A
Preparation method of corrosion-resistant aluminum alloy material containing gadolinium and yttrium
CN108048707A
Modified aluminum alloy for distribution network connection fitting and preparation method of modified aluminum alloy
CN117778909A