High-strength and high-thermal-conductivity magnesium alloy, rolled plate and preparation method of rolled plate
Through the Mg99-xZnxGdyY1-y system magnesium alloy and staged rolling process, the problem of difficulty in taking into account the strength and thermal conductivity of magnesium alloy is solved, and the preparation of high-strength and high-thermal conductivity of magnesium alloy sheets is achieved, and the poor plasticity of magnesium alloys is overcome. Rolling process limitations.
Patent Information
- Application Number
- CN202410976047.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing magnesium alloys are difficult to take into account both strength and thermal conductivity, and their own plasticity is poor, which limits the development and application of its rolling process.
Using Mg99-xZnxGdyY1-y high-strength and high-thermal conductivity magnesium alloy, through solid solution treatment and staged rolling process, Gd and Y elements in the alloy exist in the form of precipitation phases, and each pass and total down pressure during the rolling process is optimized. to ensure the strength and thermal conductivity of the material are matched.
It achieves a balance of high strength and high thermal conductivity, overcomes the limitations of moldability and mechanical properties of magnesium alloys in the rolling process, and can obtain well-formed high-strength, high-thermal conductivity magnesium alloy sheets with good molding using ordinary rolling mills.
Smart Images

Figure CN119061302A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of magnesium alloys, and in particular to a high-strength and high-thermal-conductivity magnesium alloy, a rolled plate and a preparation method thereof. Background Art
[0002] As the lightweight field develops towards multi-function and high efficiency, highly integrated electronic components and high-efficiency heat exchange devices have a wider range of application needs. The heat generated by these devices during operation needs to be discharged in time to ensure the stability of equipment operation. As the common frame structure and load-bearing part of these devices, the plate has higher requirements for its lightness, high strength and high thermal conductivity.
[0003] As the lightest metal structural material, magnesium has high specific strength, high specific stiffness and good electrical and thermal conductivity, and is expected to be used in the preparation of lightweight, high-strength and high-thermal conductivity plates. However, the low strength of pure magnesium limits its application, and alloying is currently the main method to improve its strength. However, existing magnesium alloys have problems with incompatibility between strength and thermal conductivity, and the poor plasticity of magnesium alloys limits the development of their rolling process. Summary of the invention
[0004] In response to one or more technical problems existing in the prior art, the present invention provides a high-strength and high-thermal conductivity magnesium alloy, a rolled plate and a preparation method thereof. The magnesium alloy provided by the present invention has both high strength and high thermal conductivity, overcoming the problem that the existing magnesium alloys cannot take both strength and thermal conductivity into account.
[0005] In a first aspect, the present invention provides a high-strength and high-thermal-conductivity magnesium alloy, wherein the chemical formula of the magnesium alloy is Mg 99- x Zn x G y Y 1-y , where x is 1.5 to 2 and y is not 0.
[0006] Preferably, the magnesium alloy is obtained by smelting raw materials including pure magnesium, pure zinc, magnesium-gadolinium master alloy and magnesium-yttrium master alloy.
[0007] Preferably, gadolinium accounts for 25-30wt% in the magnesium-gadolinium master alloy; and / or
[0008] The yttrium in the magnesium-yttrium master alloy accounts for 25-30wt%.
[0009] The present invention further provides a method for preparing a rolled plate in a second aspect, using the magnesium alloy described in the first aspect as a raw material, and the preparation method comprises:
[0010] The magnesium alloy is subjected to a solid solution treatment and rolling to obtain a rolled plate;
[0011] The rolling includes first rolling, second rolling and third rolling with the pressing amount increasing in each pass;
[0012] The pressing amount of each pass in the first rolling process is not more than 15%, and the total pressing amount is not less than 50%;
[0013] The pressing amount of each pass in the second rolling process is not more than 40%, and the total pressing amount is not less than 75%;
[0014] The pressing amount of each pass in the third rolling process is not more than 50%, and the total pressing amount is not less than 85%.
[0015] Preferably, the temperature of the solution treatment is 480-510° C. and the time is 10-14 hours.
[0016] Preferably, the pressing amount of each pass in the first rolling process is 10-15%;
[0017] The pressing amount of each pass in the second rolling process is 20-40%; and / or
[0018] The pressing amount of each pass in the third rolling process is 40-50%.
[0019] Preferably, the rolling temperature is 430-460°C;
[0020] The rolling speed is 15 to 25 m / min; and / or
[0021] The insulation time between the rolling passes is 7 to 12 minutes.
[0022] Preferably, an aging treatment step is further included after the rolling.
[0023] Preferably, the temperature of the aging treatment is 160-250°C;
[0024] The aging treatment time is 1 to 4 hours.
[0025] The present invention further provides a rolled plate in a third aspect, which is prepared by the preparation method described in the second aspect.
[0026] Compared with the prior art, the present invention has at least the following beneficial effects:
[0027] The present invention uses Mg-Zn alloy as the basis to ensure that the material has high thermal conductivity, and improves the mechanical properties of the alloy by introducing rare earth elements, thereby improving the strength of the magnesium alloy. At the same time, by controlling the content of alloy elements in the magnesium alloy, the Gd and Y elements exist in the form of precipitation phases, ensuring that the strength of the magnesium alloy is improved while maintaining high thermal conductivity. The magnesium alloy provided by the present invention has both high strength and high thermal conductivity, overcoming the problem that the strength and thermal conductivity of the existing magnesium alloy cannot be taken into account at the same time.
[0028] The present invention optimizes the rolling process of magnesium alloy based on the composition of magnesium alloy, and performs rolling in stages: in the first stage, a small pressing amount is used for each pass to ensure formability, and to a certain extent, the coarse grains in the solid solution state are refined; in the second stage, the pressing amount is increased for each pass to provide a driving force for subsequent recrystallization and grain refinement, and sufficient dislocation pile-up is introduced; in the third stage, a large pressing amount is used to improve the strength of the material. The present invention adjusts the microstructure of the alloy by rolling in stages and adjusting the pressing amount for each pass and the total pressing amount in each stage of the rolling process in stages, so as to achieve matching of strength, plasticity and thermal conductivity. The rolling process provided by the present invention can achieve good formability of magnesium alloy sheet by using an ordinary rolling mill (roller does not have a heating function), and obtain a magnesium alloy sheet with high strength and high thermal conductivity, which overcomes the problem that the existing magnesium alloy has limited its rolling process due to its poor plasticity, and it is difficult to take into account both high formability and high mechanical properties of magnesium alloy sheet by using an ordinary rolling mill. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a flow chart of a method for preparing a magnesium alloy rolled plate provided by the present invention;
[0031] Figure 2 The Mg provided by the present invention 97 Zn2Gd 0.5 Y 0.5 SEM image of the alloy as cast;
[0032] Figure 3 The Mg provided by the present invention 97 Zn2Gd 0.5 Y 0.5 SEM image of alloy in solid solution state;
[0033] Figure 4 Mg in Examples 1 and 2 of the present invention 97 Zn2Gd 0.5 Y 0.5 Physical picture of the alloy in the rolled state (① in the figure corresponds to Example 1, and ② in the figure corresponds to Example 2);
[0034] Figure 5 Mg in Example 1 of the present invention 97 Zn2Gd 0.5 Y 0.5Optical microscope (OM) photograph of the alloy in the aged state;
[0035] Figure 6 Mg in Example 2 of the present invention 97 Zn2Gd 0.5 Y 0.5 Optical microscope (OM) photograph of the alloy in the aged state;
[0036] Figure 7 Mg in Examples 1 and 2 of the present invention 97 Zn2Gd 0.5 Y 0.5 Tensile test results of the alloy in the aged state. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0038] In a first aspect, the present invention provides a high-strength and high-thermal-conductivity magnesium alloy, wherein the chemical formula of the magnesium alloy is Mg 99- x Zn x G y Y 1-y , where x is 1.5 to 2 and y is not 0.
[0039] It should be noted that the subscript of an element in a chemical formula represents the atomic percentage of the element.
[0040] The present invention uses Mg-Zn alloy as the basis to ensure that the material has high thermal conductivity, and improves the mechanical properties of the alloy by introducing rare earth elements, thereby improving the strength of the magnesium alloy. At the same time, by controlling the content of alloy elements in the magnesium alloy, the Gd and Y elements exist in the form of precipitation phases, ensuring that the strength of the magnesium alloy is improved while maintaining high thermal conductivity. The magnesium alloy provided by the present invention has both high strength and high thermal conductivity, overcoming the problem that the strength and thermal conductivity of the existing magnesium alloy cannot be taken into account at the same time.
[0041] Pure magnesium has a high thermal conductivity (158W / (m·K)), but due to the low strength of pure magnesium, it needs to be improved by alloying. However, with the introduction of alloying elements, different degrees of lattice distortion will occur inside the pure magnesium matrix, which will eventually lead to different degrees of reduction in the thermal conductivity of the magnesium alloy. With the increase of the content of alloying elements, the thermal conductivity of the magnesium alloy continues to decrease. The inventors found that different types of alloying elements will also have different effects on the thermal conductivity of magnesium alloys. When the same amount of alloying elements is added, the Zn element has a smaller degree of reduction in the thermal conductivity of the magnesium alloy, while heavy rare earth elements (such as Gd, Y) will significantly reduce the thermal conductivity of the magnesium alloy. When the alloying elements exist in the form of solid solution, the degree of reduction in the thermal conductivity of the magnesium alloy will be significantly higher than the degree of reduction in the thermal conductivity of the magnesium alloy when they exist in the form of precipitation phase. The premise for maintaining the high thermal conductivity of magnesium alloys is to maintain the internal alloying element content at a low level by adjusting the ratio of alloying elements so that the alloying elements exist in the form of precipitation phase as much as possible, thereby reducing the content of solid solution atoms in the matrix. Therefore, the present invention controls the content of the alloy elements within the above range.
[0042] According to some preferred embodiments, the magnesium alloy is obtained by smelting raw materials including pure magnesium, pure zinc, magnesium-gadolinium master alloy and magnesium-yttrium master alloy.
[0043] According to some preferred embodiments, the smelting process of the magnesium alloy includes: adding pure magnesium at 640-680°C in a protective atmosphere, and after it is completely melted, adding pure Zn, Mg-Gd master alloy and Mg-Y master alloy in sequence, and after it is completely melted, heating to 770-790°C and standing for 20-30 minutes to remove the surface oxide layer to obtain a mixed melt. The mixed melt is poured into a preheated mold to obtain a magnesium alloy (cast alloy).
[0044] It should be noted that the oxide layer on the surface of the melt must be removed before adding each raw material. After each raw material is added, it must be completely melted and the elements must be evenly diffused inside the melt before the next raw material can be added. Heat the mold to 250-300°C, spray the release agent evenly on the inside of the mold, and keep the mold at 250-300°C to obtain a preheated mold.
[0045] According to some specific implementation methods, the smelting process of the magnesium alloy includes: adding pure magnesium at 660°C in a protective atmosphere, and after it is completely melted, adding pure Zn, Mg-30wt.%Gd and Mg-30wt.%Y in sequence, removing the oxide layer on the surface of the melt before adding each raw material, and waiting for each raw material to be completely melted after being added, and ensuring that the elements are evenly diffused inside the melt, and then adding the next raw material. After the last raw material is added, keep it warm for 15 minutes, remove the oxide layer on the surface of the melt, stir for 5 to 10 minutes, heat it to 780°C and let it stand for 20 to 30 minutes to obtain a mixed melt. The mixed melt is cooled by pouring cooling method, the mold is preheated to 250°C, and the release agent is evenly sprayed on the inside of the mold, and the mold is kept warm at 300°C. After the mixed melt is left to stand, remove the surface oxide layer and pour it into the preheated mold to obtain a magnesium alloy (cast alloy).
[0046] According to some preferred embodiments, gadolinium accounts for 25-30 wt % (for example, 25 wt %, 26 wt %, 27 wt %, 28 wt %, 29 wt % or 30 wt %) in the magnesium-gadolinium master alloy.
[0047] According to some preferred embodiments, yttrium accounts for 25-30 wt % (for example, 25 wt %, 26 wt %, 27 wt %, 28 wt %, 29 wt % or 30 wt %) in the magnesium-yttrium master alloy.
[0048] The present invention further provides a method for preparing a rolled plate in a second aspect, using the magnesium alloy described in the first aspect as a raw material, and the preparation method comprises:
[0049] The magnesium alloy is subjected to a solid solution treatment and rolling to obtain a rolled plate;
[0050] The rolling includes first rolling, second rolling and third rolling with the pressing amount increasing in each pass;
[0051] The pressing amount of each pass in the first rolling process is not more than 15%, and the total pressing amount is not less than 50%;
[0052] The pressing amount of each pass in the second rolling process is not more than 40%, and the total pressing amount is not less than 75%;
[0053] The pressing amount of each pass in the third rolling process is not more than 50%, and the total pressing amount is not less than 85%.
[0054] Due to the poor plasticity of magnesium alloys, edge cracks are prone to occur during the rolling process. Severe edge cracks will deteriorate the mechanical properties of the alloy and even cause the sheet to fail. Therefore, the formability of the sheet must be considered when preparing the magnesium alloy rolled sheet. In order to maintain good mechanical properties of the rolled magnesium alloy sheet, the rolling temperature cannot be too high, and the pressure per pass and the total pressure cannot be too low. However, this will aggravate the cracking tendency of the magnesium alloy sheet during the rolling process. It is often necessary to use a rolling mill with a heating function to achieve the forming of the magnesium alloy sheet. Ordinary rolling mills are difficult to achieve both high formability and high mechanical properties of magnesium alloy sheets, which greatly limits the development and application of magnesium alloy rolling.
[0055] Existing magnesium alloy rolling is usually multi-pass hot rolling, in which the rolling temperature, the amount of pressure per pass, the total amount of pressure and the rolling speed have a great influence on the performance of the material. The inventor found that at a relatively low temperature, or using a large amount of pressure per pass (≥20%) helps the material to obtain a higher strength, but it is very easy to cause edge cracks in the material, and it is impossible to achieve a higher cumulative pressure, and the plasticity of the material is greatly reduced. Although increasing the temperature or using a smaller amount of pressure per pass (≤10%) can improve the formability of the sheet, it is easy to make the final structure coarse grains, insufficient work hardening ability, and poor mechanical properties. Although using a warm rolling mill to heat the rollers to a certain temperature can improve the rollability of the magnesium alloy sheet, it has high requirements on the equipment. Based on this, the present invention provides a rolling process for rolling magnesium alloy sheets using a traditional hot rolling method (rollers are not heated and lubricated) to ensure that magnesium alloys can be universally applicable on various rolling mills.
[0056] The present invention optimizes the rolling process of magnesium alloy based on the composition of magnesium alloy, and performs rolling in stages: in the first stage, a small pressing amount is used for each pass to ensure formability, and to a certain extent, the coarse grains in the solid solution state are refined; in the second stage, the pressing amount is increased for each pass to provide a driving force for subsequent recrystallization and grain refinement, and sufficient dislocation pile-up is introduced; in the third stage, a large pressing amount is used to improve the strength of the material. The present invention adjusts the microstructure of the alloy by rolling in stages and adjusting the pressing amount for each pass and the total pressing amount in each stage of the rolling process in stages, so as to achieve matching of strength, plasticity and thermal conductivity. The rolling process provided by the present invention can achieve good formability of magnesium alloy sheet by using an ordinary rolling mill (roller does not have a heating function), and obtain a magnesium alloy sheet with high strength and high thermal conductivity, which overcomes the problem that the existing magnesium alloy has limited its rolling process due to its poor plasticity, and it is difficult to take into account both high formability and high mechanical properties of magnesium alloy sheet by using an ordinary rolling mill.
[0057] According to some preferred embodiments, the solution treatment is performed at a temperature of 480-510°C (for example, 480°C, 490°C, 500°C or 510°C) and for a time of 10-14h (for example, 10h, 11h, 12h, 13h or 14h).
[0058] According to some preferred embodiments, the pressing amount of each pass in the first rolling process is 10-15% (for example, 10%, 11%, 12%, 13%, 14% or 15%).
[0059] According to some preferred embodiments, the pressing amount of each pass in the second rolling process is 20-40% (for example, 20%, 25%, 30%, 35% or 40%).
[0060] According to some preferred embodiments, the amount of pressing in each pass of the third rolling process is 40-50% (for example, it can be 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49% or 50%).
[0061] According to some preferred embodiments, the rolling temperature is 430-460° C. (for example, 430° C., 440° C., 450° C. or 460° C.).
[0062] According to some preferred embodiments, the rolling speed is 15 to 25 m / min (for example, it can be 15 m / min, 16 m / min, 17 m / min, 18 m / min, 19 m / min, 20 m / min, 21 m / min, 22 m / min, 23 m / min, 24 m / min or 25 m / min).
[0063] According to some preferred embodiments, the holding time between rolling passes is 7 to 12 minutes (for example, it may be 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes or 12 m / min).
[0064] According to some preferred embodiments, the step of performing aging treatment is further included after the rolling. The present invention further optimizes the comprehensive properties of the alloy through aging treatment after the rolling is completed.
[0065] According to some preferred embodiments, the temperature of the aging treatment is 160-250°C (for example, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C or 250°C);
[0066] The aging treatment time is 1 to 4 hours (for example, 1 hour, 2 hours, 3 hours or 4 hours).
[0067] The present invention further provides a rolled plate in a third aspect, which is prepared by the preparation method described in the second aspect.
[0068] In order to more clearly illustrate the technical solutions and advantages of the present invention, the present invention is further described below in conjunction with the examples. The present invention does not specifically limit the sources of the reagents used in the examples and comparative examples, and the reagents can be directly purchased or synthesized by themselves.
[0069] Example 1
[0070] A high-strength and high-thermal-conductivity magnesium alloy, whose chemical formula is Mg 97 Zn2Gd 0.5 Y 0.5 ; The preparation method of the alloy includes: firstly heating the resistance furnace to 760°C, then placing the crucible and introducing the protective gas, which is a mixture of CO2 and SF6, wherein the volume fraction of SF6 is 2.4vol.%; when the temperature of the crucible rises to 660°C, adding pure magnesium and waiting for it to be completely melted, preheating pure Zn, Mg-30wt.%Gd and Mg-30wt.%Y at 250°C, and after the pure magnesium is completely melted, adding pure Zn, Mg-30wt.%Gd and Mg-30wt.%Y in sequence. Before adding each raw material, the oxide layer on the surface of the melt in the crucible needs to be scraped off, and then the raw material is clamped with a clamp and slowly placed in the melt. After each raw material is placed in the crucible, it needs to wait for about 15 minutes to make it completely melted, and ensure that the elements are evenly diffused in the melt. The next raw material can be added only after the previous raw material has been diffused.
[0071] After the last raw material is added, keep the temperature for 15 minutes, then remove the oxide layer on the surface of the melt, stir for 5 to 10 minutes, and after stirring, heat the resistance furnace to 780°C and let it stand for 20 to 30 minutes. The melt is cooled by pouring cooling method. The mold is preheated to 250°C, and then the release agent is evenly sprayed on the inside of the mold, and then the mold is kept at 300°C. After the melt is left to stand, remove the surface oxide layer, and then immediately pour the melt in the crucible into the preheated mold to obtain a magnesium alloy (cast alloy). The obtained magnesium alloy ingot is processed into a 45×30×8mm rectangular thick plate by wire cutting, and a chamfer is prefabricated on the short side of one side of the rectangle to facilitate subsequent rolling.
[0072] A method for preparing a rolled plate, comprising:
[0073] First, Mg 97 Zn2Gd 0.5 Y 0.5 The alloy was subjected to a solution treatment at a temperature of 500°C for 12 hours. Then, the Mg after the solution treatment was rolled using a conventional rolling mill. 97 Zn2Gd 0.5 Y0.5 The alloy is rolled, and the rolling process includes: first, 6 passes of small pressing amount rolling, each pass has a pressing amount of 10%, at this time the total pressing amount reaches 50%, then 1 pass of 20% pressing amount rolling is performed, and then 1 pass of 37.5% pressing amount rolling is performed, at this time the total pressing amount reaches 75%. Finally, the final pass of 50% pressing amount rolling is performed, at this time the total pressing amount of the plate reaches 87.5%, the rolling temperature of the whole rolling process is 450℃, the rolling speed is 20m / min, and the heat preservation between rolling passes is 10min. After the rolling is completed, the rolled plate is subjected to aging treatment, wherein the aging treatment temperature is 200℃ and the time is 2h to obtain a rolled plate.
[0074] In this embodiment, Mg 97 Zn2Gd 0.5 Y 0.5 The main precipitated phase in the cast alloy is a network of W phase (Mg3Zn3RE2), such as Figure 2 , after solution treatment, the network W phase is transformed into spherical W phase, such as Figure 3 The network eutectic phase easily causes crack initiation and expansion during the deformation of magnesium alloys. Solution treatment can make the material composition uniform and avoid the adverse effects of the network W phase, thereby improving the subsequent rolling formability and final comprehensive mechanical properties of the material.
[0075] Example 2
[0076] It is basically the same as Example 1, except that:
[0077] A method for preparing a rolled plate, comprising:
[0078] First, Mg 97 Zn2Gd 0.5 Y 0.5 The alloy was subjected to a solution treatment at a temperature of 500°C for 12 hours. Then, the Mg after the solution treatment was rolled using a conventional rolling mill. 97 Zn2Gd 0.5 Y 0.5 The alloy is rolled, and the rolling process includes: first, 6 passes of small pressing amount rolling, each pass of pressing amount is 10%, at this time the total pressing amount reaches 50%; then 3 passes of 20% pressing amount rolling, at this time the total pressing amount reaches 75%; finally, the final pass of 50% pressing amount rolling, at this time the total pressing amount of the plate reaches 87.5%, the rolling temperature of the whole rolling process is 450℃, the rolling speed is 20m / min, and the heat preservation between the rolling passes is 10min. After the rolling is completed, the rolled plate is subjected to aging treatment, wherein the aging treatment temperature is 200℃, the time is 2h, and the rolled plate is obtained.
[0079] The thickness changes during the rolling process of Example 1 and Example 2 of the present invention are shown in Table 1.
[0080] Table 1. Thickness changes during rolling process of Example 1 and Example 2 of the present invention
[0081]
[0082] The rolled plates obtained in Example 1 and Example 2 have excellent formability, and almost no edge cracking occurs in the plates. Figure 4 After rolling, Example 1 and Example 2 were subjected to aging treatment to obtain the final microstructure, as shown in FIG. Figure 5-6 (In the figure, RD is the rolling direction, ND is the normal direction, and TD is the transverse direction). The microstructures of the rolled plates prepared by the two embodiments are relatively close, showing a typical bi-modal structure composed of large-sized deformed grains and fine recrystallized grains, and the spheroidized W phase is distributed along the RD direction (rolling direction).
[0083] Depend on Figure 7 It can be seen that the Mg prepared in Example 1 and Example 2 97 Zn2Gd 0.5 Y 0.5 The tensile stress-strain curve of the alloy rolled plate at room temperature shows that the materials prepared in Example 1 and Example 2 show good comprehensive mechanical properties, with a yield strength of >250MPa and an elongation at break of >15%. The mechanical properties of the material are closely related to the microstructure. The dual-mode structure can provide the material with better mechanical properties. The dislocation accumulation inside the large deformed grains can hinder the dislocation slip and improve the material strength. The fine recrystallized grains can coordinate the deformation and improve the plasticity of the material. According to the Hall-Patch law, small-sized recrystallized grains can also contribute to the strength of the material through grain boundary strengthening. In addition, the spheroidized W phase can also hinder the dislocation slip to a certain extent, playing the role of second phase strengthening. Therefore, the Mg prepared in Example 1 and Example 2 of the present invention 97 Zn2Gd 0.5 Y 0.5 Alloy rolled plates have good strength and plasticity.
[0084] Example 3
[0085] It is basically the same as Example 1, except that no aging treatment is performed after rolling.
[0086] Comparative Example 1
[0087] It is basically the same as Example 3, except that the chemical formula of the high-strength and high-thermal-conductivity magnesium alloy is Mg 98 Zn1Gd 0.5 Y 0.5 .
[0088] Comparative Example 2
[0089] It is basically the same as Example 3, except that the chemical formula of the high-strength and high-thermal-conductivity magnesium alloy is Mg 98.33 Zn 0.67 G 0.5 Y 0.5 .
[0090] The actual chemical composition of the magnesium alloy (cast alloy) involved in the embodiments and comparative examples of the present invention is shown in Table 2.
[0091] Table 2. Actual chemical composition of magnesium alloys (cast alloys) involved in the embodiments of the present invention and comparative examples
[0092]
[0093]
[0094] It should be noted that RE in the present specification is a rare earth metal, and RE / Zn represents the atomic ratio of the rare earth metal to zinc.
[0095] Comparative Example 3
[0096] The method is basically the same as Example 1, except that the rolling process includes: the pressing amount of each pass is 10%, and a total of 14 passes are performed to roll the initial 8 mm thick plate into a 1.6 mm thick thin plate, at which the total pressing amount is 80%. The rolling temperature of the entire rolling process is 450°C, the rolling speed is 20 m / min, and the heat preservation is 10 minutes between rolling passes.
[0097] Comparative Example 4
[0098] It is basically the same as Example 1, except that the rolling process includes: the pressing amount in each pass is 20%, the rolling temperature of the whole rolling process is 450°C, the rolling speed is 20m / min, and the insulation between rolling passes is 10min.
[0099] The inventors found that after 4 rolling passes, the plate had severe edge cracks, and after 5 rolling passes, the cracks expanded rapidly inward, making it difficult for the plate to meet the formability requirements.
[0100] Comparative Example 5
[0101] The method is basically the same as Example 1, except that the rolling process includes: firstly, rolling with a 10% reduction in each pass, and after three passes of rolling, the total reduction in the plate reaches 30%, and then rolling with a 20% reduction in each pass, and after three passes of rolling, the total reduction in the plate reaches 70%. The rolling temperature of the entire rolling process is 450°C, the rolling speed is 20m / min, and the heat preservation is 10min between rolling passes.
[0102] The inventors found that after three passes of rolling with a 10% reduction, the plate had good formability, but after three passes of rolling with a 20% reduction, the plate had severe edge cracks, and the cracks expanded inward.
[0103] Comparative Example 6
[0104] The method is basically the same as Example 1, except that the rolling process includes: firstly, rolling with a 10% reduction in each pass, and after 6 passes, the total reduction in the plate reaches 50%; then, rolling with a 50% reduction in the final pass, and the total reduction in the plate reaches 75%. The rolling temperature of the entire rolling process is 450°C, the rolling speed is 20m / min, and the heat preservation is 10min between rolling passes.
[0105] The inventors found that after 6 passes of rolling with a 10% reduction, the plate had good formability, but after the final pass of rolling with a 50% reduction, the plate was severely broken.
[0106] Comparative Example 7
[0107] The method is basically the same as Example 1, except that: first, a rolling process with a 10% reduction is performed, and after 6 rolling processes, the total reduction of the plate reaches 50%; then a rolling process with a 20% reduction is performed, and the total reduction of the plate reaches 60%; finally, a final rolling process with a 50% reduction is performed, and the total reduction of the plate reaches 80%. The rolling temperature of the entire rolling process is 450°C, the rolling speed is 20m / min, and the heat preservation is performed for 10 minutes between rolling processes.
[0108] The inventors found that the plate was severely broken after rolling with a 50% reduction in the final pass.
[0109] Comparative Example 8
[0110] The method is basically the same as Example 1, except that the rolling process includes: firstly, rolling with a 10% reduction in each pass, and after 10 passes, the total reduction in the plate reaches 70%, and then rolling with a 50% reduction in the final pass, at which time the total reduction in the plate reaches 85%. The rolling temperature of the entire rolling process is 450°C, the rolling speed is 20m / min, and the heat preservation is 10min between rolling passes.
[0111] The inventors found that the sheet has good formability, but poor mechanical properties and extremely low elongation.
[0112] The test results of the properties of the magnesium alloy rolled plates of the embodiments of the present invention and the comparative examples are shown in Table 3.
[0113] Table 3. Mechanical and thermal conductivity properties of magnesium alloy rolled plates obtained in the embodiments of the present invention and the comparative examples
[0114]
[0115] It should be noted that, due to poor formability and failure of the plates in comparative examples 4-7, relevant performance tests were not conducted, and the “-” in comparative example 8 indicates that relevant tests were not conducted.
[0116] It can be seen from Table 3 that the materials prepared in Examples 1-3 of the present invention have good thermal conductivity while taking into account both strength and plasticity, meeting the performance requirements of high thermal conductivity magnesium alloys. Among them, the room temperature thermal conductivity of Example 1 and Example 2 is >120 W / (m·K), indicating that aging treatment can promote the generation of precipitation phases inside the alloy or reduce dislocation density to improve the thermal conductivity of the deformed magnesium alloy, thereby further improving the thermal conductivity of the material.
[0117] From the thermal conductivity of the magnesium alloy plates prepared in Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that as the RE / Zn ratio increases, the main alloying element in magnesium changes from Zn to RE, and the thermal conductivity of the alloy shows a significant downward trend. The reason is that on the one hand, the degree of reduction of the thermal conductivity of magnesium by the same content of Zn is significantly lower than that of the same content of RE, and on the other hand, the reduction of Zn content significantly reduces the content of precipitated phases that can be formed in the alloy, and the content of RE elements in the form of solid solution atoms increases. Mg in Example 1 97 Zn2Gd 0.5 Y 0.5 The atomic ratio of RE / Zn in the alloy is 2.0, which can form a large amount of W phase (Mg3Zn3RE2) inside the alloy. This precipitated phase can reduce the content of Zn and RE dissolved in the matrix, which is beneficial to the thermal conductivity of the alloy, and can also provide strengthening effect in terms of mechanical properties.
[0118] In summary, the present invention is based on Mg-Zn alloy to ensure that the material has high thermal conductivity, and improves the mechanical properties of the alloy by introducing rare earth elements, thereby improving the strength of the magnesium alloy. At the same time, by controlling the content of alloying elements in the magnesium alloy, Gd and Y elements exist in the form of precipitated phases, ensuring that the strength of the magnesium alloy is improved while maintaining a high thermal conductivity. The present invention optimizes the rolling process of the magnesium alloy based on the composition of the magnesium alloy, and adjusts the microstructure of the alloy by rolling in stages and adjusting the pressing amount and the total pressing amount in each stage of the rolling process in stages, so as to achieve the matching of strength, plasticity and thermal conductivity. The rolling process provided by the present invention can achieve good formability of the magnesium alloy sheet by using an ordinary rolling mill (the rolling roller does not have a heating function), and obtain a magnesium alloy sheet with high strength and high thermal conductivity, which overcomes the problem that the existing magnesium alloy has limited its rolling process due to its poor plasticity, and it is difficult to take into account the high formability and high mechanical properties of the magnesium alloy sheet by using an ordinary rolling mill.
[0119] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high-strength and high-thermal-conductivity magnesium alloy, It is characterized in that The chemical formula of the magnesium alloy is Mg 99-x Zn x G y Y 1-y , where x is 1.5 to 2 and y is not 0.
2. The magnesium alloy according to claim 1, It is characterized in that The magnesium alloy is obtained by smelting raw materials including pure magnesium, pure zinc, magnesium-gadolinium master alloy and magnesium-yttrium master alloy.
3. The magnesium alloy according to claim 2, It is characterized in that The magnesium-gadolinium master alloy contains 25-30 wt% gadolinium; and / or The yttrium in the magnesium-yttrium master alloy accounts for 25-30wt%.
4. A method for preparing a rolled plate, It is characterized in that Using the magnesium alloy according to any one of claims 1 to 3 as a raw material, the preparation method comprises: The magnesium alloy is subjected to solution treatment and rolling to obtain a rolled plate; The rolling includes first rolling, second rolling and third rolling with the pressing amount increasing in each pass; The pressing amount of each pass in the first rolling process is not more than 15%, and the total pressing amount is not less than 50%; The pressing amount of each pass in the second rolling process is not more than 40%, and the total pressing amount is not less than 75%; The pressing amount of each pass in the third rolling process is not more than 50%, and the total pressing amount is not less than 85%.
5. The preparation method according to claim 4, It is characterized in that The temperature of the solution treatment is 480-510° C. and the time is 10-14 hours.
6. The preparation method according to claim 4, It is characterized in that The pressing amount of each pass in the first rolling process is 10-15%; The pressing amount of each pass in the second rolling process is 20-40%; and / or The pressing amount of each pass in the third rolling process is 40-50%.
7. The preparation method according to claim 4, It is characterized in that The rolling temperature is 430-460°C; The rolling speed is 15 to 25 m / min; and / or The insulation time between the rolling passes is 7 to 12 minutes.
8. The preparation method according to claim 4, It is characterized in that After the rolling, an aging treatment step is also included.
9. The preparation method according to claim 8, It is characterized in that The aging treatment temperature is 160-250°C; and / or The aging treatment time is 1 to 4 hours.
10. A rolled plate, It is characterized in that The method is prepared by the preparation method according to any one of claims 4 to 9.
Citation Information
Patent Citations
Hot rolling process of high-plasticity and low-anisotropy magnesium alloy and sheet thereof
CN101857933A
Ultrahigh-strength rare earth-magnesium alloy board and preparation method thereof
CN102337441A
Efficient rolling method for magnesium alloy plate with weak and non-base-surface texture
CN106995908A
High-speed extruded magnesium alloy deformed profile low in rare earth content and preparation technique thereof
CN107012376A
Casting magnesium alloy and preparation method thereof
CN107354355A