High-performance die-casting die steel material and preparation process thereof
A high-performance die-casting mold steel material with tailored alloy elements addresses thermal conductivity and mold life issues, enabling crack-free SLM production and cost-effective, high-quality die-casting.
Patent Information
- Application Number
- CN202411213210.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-12-03
AI Technical Summary
Existing die-casting mold materials, particularly those made from 18Ni300, suffer from low thermal conductivity, poor heat resistance, and short mold life due to thermal fatigue cracking, leading to mold sticking and reduced product quality, with SLM technology facing challenges in producing large molds without cracks at high substrate heating temperatures.
A high-performance die-casting mold steel material composed of specific alloy elements (e.g., Co, Ni, Mo, Cr, Si, Mn, C, V, and Fe) is developed, processed into spherical powders, and optimized using SLM equipment with controlled heat treatment to achieve crack-free printing and improved thermal conductivity, meeting equipment heating requirements and reducing production costs.
The new material enables crack-free, high-density printing at 180°C substrate heating, enhancing mold life, accelerating cycle times, and improving product quality with better mechanical properties compared to traditional carbon steel powders.
Smart Images

Figure CN119061332A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of mold material preparation, in particular to a high-performance die-casting mold steel material and a preparation process thereof. Background Art
[0002] In order to reduce the problem of large molds being replaced as a whole due to local failure, the mode of block inserts is adopted for combination. Insufficient cooling speed and uneven cooling at the pouring and deep cavity locations can easily lead to mold sticking and meat loss in die-casting products. The additive manufacturing selective laser melting (SLM) technology can produce conformal water channel molds to solve this problem. Therefore, additive manufacturing technology is widely used in the production of mold inserts at the core and mold core, effectively improving the life of the mold.
[0003] SLM technology is currently widely used in molds, automobiles and other fields. Selective Laser Melting (SLM) is a powder bed-based laser melting technology. This technology produces metal parts with complex structures by stacking metal powder layer by layer and melting it with a high-energy laser beam. The advantage of SLM technology is that it can produce parts with complex geometries without the need for molds, which greatly reduces manufacturing costs and time. The die-casting mold formed by SLM has a complex conformal cooling water channel, which can greatly shorten the die-casting cycle and improve product quality, but the life of the mold often cannot meet actual needs.
[0004] 18Ni300 is the most widely used mold steel material for SLM. It has low thermal conductivity and poor heat resistance. In actual production, the mold life is short, which easily leads to mold sticking of die-casting products and low product quality. A more comprehensive SLM die-casting mold material is needed to solve these problems.
[0005] Due to the characteristics of SLM technology, such as rapid cooling and heating and high molten pool temperature (above 2500℃), traditional carbon steel hot working die steel powder (H13, Dievar) needs to be heated at a high temperature of the substrate of the additive manufacturing equipment to be formed without cracking. This greatly increases the production cost and difficulty of the equipment and limits the production size of the mold. It is necessary for the material to be able to be formed in large sizes without cracks at the substrate heating temperature that can be provided by the current SLM equipment. Summary of the invention
[0006] In view of the problems in the related technology, the present invention proposes a high-performance die-casting mold steel material and its preparation process to overcome the above-mentioned technical problems existing in the existing related technology. The purpose of the present invention is to adjust the types of alloy elements in carbon steel so that it can achieve crack-free printing and forming under the condition of 180°C substrate heating, meet the heating indicators of current equipment and leave a margin; lower cost, and have good thermal conductivity, can accelerate the cycle time of die-casting production, and improve product quality; have good mechanical properties, which are significantly better than traditional carbon steel powder for SLM.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] A high-performance die-casting mold steel material comprises the following components by weight: 0.5-0.8% cobalt, 0.4-0.7% nickel, 2.8-4.2% molybdenum, 4.5-5.5% chromium, 0.1-0.15% silicon, 0.4-0.65% manganese, 0.3-0.45% carbon, 0.4-0.7% vanadium and 84-92% iron.
[0009] Preferably, the following components are included by weight: 0.6% cobalt, 0.5% nickel, 2.9% molybdenum, 4.8% chromium, 0.12% silicon, 0.4% manganese, 0.3% carbon, 0.4% vanadium and 89.98% iron.
[0010] Preferably, the following components are included in weight percentage: 0.8% cobalt, 0.7% nickel, 4.2% molybdenum, 5.5% chromium, 0.15% silicon, 0.65% manganese, 0.45% carbon, 0.7% vanadium and 86.85% iron.
[0011] Preferably, the following components are included by weight: 0.8% cobalt, 0.6% nickel, 3.8% molybdenum, 4.7% chromium, 0.12% silicon, 0.55% manganese, 0.43% carbon, 0.6% vanadium and 88.4% iron.
[0012] To achieve the above object, the present invention also provides the following technical solutions:
[0013] A preparation process of high-performance die-casting die steel material comprises the following steps:
[0014] S1. Weigh the raw materials of high-performance die-casting mold steel materials according to the above weight percentages, and prepare the raw materials into spherical powders by vacuum gas atomization. The powder particle size range of the additive manufacturing use state is 15-53 μm normal distribution;
[0015] S2. Prepare test specimens using selective laser melting equipment;
[0016] S3. Optimize the heat treatment system of the molded material to obtain the best heat treatment conditions and the best material properties.
[0017] Preferably, in S2, the molding parameters of the selective laser melting are: molding thickness 0.05 mm, line spacing 0.08 mm, spot size 0.01 mm, laser power 300 W, line scanning speed 1100 mm / s, substrate heating temperature 180°C.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention is a high-performance die-casting die steel material and its preparation process. The carbon steel proposed in the present invention can achieve crack-free printing and forming under the condition of 180°C substrate heating by adjusting the types of alloy elements, meeting the heating index of the current equipment and leaving a margin;
[0020] (2) The present invention is a high-performance die-casting mold steel material and its preparation process. Compared with maraging mold steel with a high alloy content, this type of carbon steel has a lower cost and good thermal conductivity, which can accelerate the cycle time of die-casting production and improve product quality; it has good mechanical properties and is significantly better than traditional carbon steel powder for SLM. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] The present invention discloses a high-performance die-casting die steel material and a preparation process thereof. To achieve the above-mentioned purpose, the present invention also provides the following technical solutions:
[0025] A high performance die casting die steel material includes the following components by weight percentage: 0.6% cobalt, 0.5% nickel, 2.9% molybdenum, 4.8% chromium, 0.12% silicon, 0.4% manganese, 0.3% carbon, 0.4% vanadium and 89.98% iron.
[0026] To achieve the above object, the present invention also provides the following technical solutions:
[0027] A preparation process of high-performance die-casting die steel material comprises the following steps:
[0028] S1. Weigh the raw materials of high-performance die-casting mold steel materials according to the above weight percentages, and prepare the raw materials into spherical powders by vacuum gas atomization. The powder particle size range of the additive manufacturing use state is 15-53 μm normal distribution;
[0029] S2. Use the selective laser melting equipment to prepare the test specimens; the molding parameters of the selective laser melting are: molding thickness 0.05 mm, line spacing 0.08 mm, spot size 0.01 mm, laser power 300 W, line scanning speed 1100 mm / s, substrate heating temperature 180 ° C;
[0030] S3. Optimize the heat treatment system of the molded material to obtain the best heat treatment conditions and the best material properties.
[0031] The materials for the additive manufacturing end of carbon steel die-casting molds are mainly Dievar and H13, which present certain challenges at the molding end of the SLM process. Crack-free production can only be guaranteed when the SLM equipment substrate is heated to 500°C, which is difficult to achieve with current production equipment and requires extremely high production costs. The problem solved by the present invention is to achieve crack-free, high-density printing of materials at the heating temperature commonly used by the equipment, as shown in Table 1 below, which can effectively reduce costs.
[0032] Even though the thermal conductivity of H13 and Dievar is higher than that of the traditional mold material 18Ni300, in actual production, thermal fatigue cracking may occur due to the brittleness of the material, resulting in mold cracking. The present invention solves the mold cracking problem and increases the service life of the mold, as shown in Table 2 below.
[0033]
[0034] Table 1
[0035]
[0036] Table 2
[0037] The Co element is added in the present invention:
[0038] 1. Promote carbide precipitation: Since Co is a non-carbide-forming element, it can be dissolved in the matrix but does not form intermetallic compounds. It can promote carbide precipitation and improve the hardness and strength of the matrix;
[0039] 2. Enhance the stability of martensite: When Co is added alone, it can increase the self-diffusion coefficient of Fe, accelerate the transformation of γ-α phase, enhance the stability of martensite, inhibit the recovery of dislocation substructure in martensite, provide more positions for the nucleation of precipitation phase, and obtain small and evenly distributed precipitation phase;
[0040] 3. Improve high temperature performance: Co can increase the Curie temperature, slow down its diffusion in the matrix, and increase the high temperature hardness of the matrix. At the same time, it can also reduce the solid solubility of Mo in the matrix, promote the precipitation of Mo-containing intermetallic compounds, and thus improve the strength and hardness of the steel.
[0041] The Co element is added in the present invention:
[0042] 1. Nickel and iron can be infinitely dissolved. Nickel expands the austenite zone of iron and is the main alloy element for forming and stabilizing austenite, improving the plasticity of the material and achieving crack-free high-density forming without high-temperature heating.
[0043] 2. The alloy elements in the material account for a relatively small proportion and have a high thermal conductivity. The type and amount of carbide precipitation can be controlled through heat treatment process to further improve the thermal conductivity of the material.
[0044] As shown in Table 3 below, the performance of the present invention was tested:
[0045]
[0046] Heat treatment conditions Impact toughness / J Sedimentary state 20 620℃ / 3h 25
[0047] After the samples of the present invention were heat treated at 620°C for 3 hours, thermal conductivity tests were performed, as shown in Table 4 below:
[0048]
[0049]
[0050] Table 4
[0051] The present invention discloses a high-performance die-casting die steel material and a preparation process thereof. The carbon steel proposed in the present invention can realize crack-free printing and forming under 180°C substrate heating conditions by adjusting the types of alloy elements, thereby meeting the heating index of current equipment and leaving a margin. Compared with martensitic aging die steel with a high alloy content, this type of carbon steel has a lower cost and good thermal conductivity, can accelerate the cycle time of die-casting production, and improve product quality. It has good mechanical properties and is significantly superior to traditional carbon steel powder for SLM.
[0052] Example 2
[0053] The present invention discloses a high-performance die-casting die steel material and a preparation process thereof. To achieve the above-mentioned purpose, the present invention also provides the following technical solutions:
[0054] A high performance die casting die steel material includes the following components by weight percentage: 0.8% cobalt, 0.7% nickel, 4.2% molybdenum, 5.5% chromium, 0.15% silicon, 0.65% manganese, 0.45% carbon, 0.7% vanadium and 86.85% iron.
[0055] To achieve the above object, the present invention also provides the following technical solutions:
[0056] A preparation process of high-performance die-casting die steel material comprises the following steps:
[0057] S1. Weigh the raw materials of high-performance die-casting mold steel materials according to the above weight percentages, and prepare the raw materials into spherical powders by vacuum gas atomization. The powder particle size range of the additive manufacturing use state is 15-53 μm normal distribution;
[0058] S2. Use the selective laser melting equipment to prepare the test specimens; the molding parameters of the selective laser melting are: molding thickness 0.05 mm, line spacing 0.08 mm, spot size 0.01 mm, laser power 300 W, line scanning speed 1100 mm / s, substrate heating temperature 180 ° C;
[0059] S3. Optimize the heat treatment system of the molded material to obtain the best heat treatment conditions and the best material properties.
[0060] Example 3
[0061] The present invention discloses a high-performance die-casting die steel material and a preparation process thereof. To achieve the above-mentioned purpose, the present invention also provides the following technical solutions:
[0062] A high performance die casting die steel material includes the following components by weight percentage: 0.8% cobalt, 0.6% nickel, 3.8% molybdenum, 4.7% chromium, 0.12% silicon, 0.55% manganese, 0.43% carbon, 0.6% vanadium and 88.4% iron.
[0063] To achieve the above object, the present invention also provides the following technical solutions:
[0064] A preparation process of high-performance die-casting die steel material comprises the following steps:
[0065] S1. Weigh the raw materials of high-performance die-casting mold steel materials according to the above weight percentages, and prepare the raw materials into spherical powders by vacuum gas atomization. The powder particle size range of the additive manufacturing use state is 15-53 μm normal distribution;
[0066] S2. Use the selective laser melting equipment to prepare the test specimens; the molding parameters of the selective laser melting are: molding thickness 0.05 mm, line spacing 0.08 mm, spot size 0.01 mm, laser power 300 W, line scanning speed 1100 mm / s, substrate heating temperature 180 ° C;
[0067] S3. Optimize the heat treatment system of the molded material to obtain the best heat treatment conditions and the best material properties.
[0068] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high performance die casting die steel material, characterized in that: It comprises the following components by weight: cobalt 0.5-0.8%, nickel 0.4-0.7%, molybdenum 2.8-4.2%, chromium 4.5-5.5%, silicon 0.1-0.15%, manganese 0.4-0.65%, carbon 0.3-0.45%, vanadium 0.4-0.7% and iron 84-92%.
2. The high performance die casting die steel material according to claim 1, characterized in that: It comprises the following components by weight: 0.6% cobalt, 0.5% nickel, 2.9% molybdenum, 4.8% chromium, 0.12% silicon, 0.4% manganese, 0.3% carbon, 0.4% vanadium and 89.98% iron.
3. The high performance die casting die steel material according to claim 1, characterized in that: It comprises the following components by weight: 0.8% cobalt, 0.7% nickel, 4.2% molybdenum, 5.5% chromium, 0.15% silicon, 0.65% manganese, 0.45% carbon, 0.7% vanadium and 86.85% iron.
4. The high performance die casting die steel material according to claim 1, characterized in that: It comprises the following components by weight: 0.8% cobalt, 0.6% nickel, 3.8% molybdenum, 4.7% chromium, 0.12% silicon, 0.55% manganese, 0.43% carbon, 0.6% vanadium and 88.4% iron.
5. A process for preparing a high performance die casting die steel material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1. Weigh the raw materials of high-performance die-casting mold steel materials according to the above weight percentages, and prepare the raw materials into spherical powders by vacuum gas atomization. The powder particle size range of the additive manufacturing state is 15-53 μm with normal distribution; S2. Prepare test specimens using selective laser melting equipment; S3. Optimize the heat treatment system of the molded material to obtain the best heat treatment conditions and the best material properties.
6. The process for preparing a high performance die casting die steel material according to claim 5, characterized in that: In S2, the molding parameters of the selective laser melting are: molding thickness 0.05 mm, line spacing 0.08 mm, spot size 0.01 mm, laser power 300 W, line scanning speed 1100 mm / s, and substrate heating temperature 180°C.