Preparation method of wear-resistant and corrosion-resistant hydrophobic titanium alloy surface with micro-nano structure

A method combining tungsten carbide imprinting, iron layer deposition, and fluorosilane treatment creates a micro-nano structured titanium carbide ceramic layer, enhancing the wear and corrosion resistance and hydrophobicity of titanium alloy surfaces, addressing the limitations of existing methods.

CN119061353AActive Publication Date: 2024-12-03XIAN UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411182075.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-03
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

Existing methods for preparing titanium alloy surfaces struggle to achieve high ceramic volume fraction and bonding strength, leading to poor wear and corrosion resistance, especially in complex marine environments, and lack sufficient hydrophobicity.

Method used

A method involving surface pretreatment with tungsten carbide particle imprinting, followed by iron layer deposition, high-temperature heat treatment, carburizing, and fluorosilane treatment to create a micro-nano structured titanium carbide ceramic layer with enhanced bonding and hydrophobic properties.

Benefits of technology

The method results in a titanium alloy surface with improved wear resistance, corrosion resistance, and hydrophobicity, achieving a microhardness of 2400HV and a water contact angle over 150°, suitable for durable use in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061353A_ABST
    Figure CN119061353A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a wear-resistant and corrosion-resistant hydrophobic titanium alloy surface with a micro-nano structure. Comprising the following steps that firstly, micron-scale pits are embossed in the pretreated titanium alloy surface through spherical tungsten carbide particles; preparing an iron layer on the surface of the titanium alloy with the pits by using a surface treatment process; then high-temperature heat treatment and carburizing treatment are carried out on the iron layer, and a titanium carbide layer with a micro-nano secondary rough structure is obtained near the interface of the iron layer and the titanium alloy; then immersing the surface into corrosive liquid to remove an iron layer on the surface; and finally, low-surface-energy modification is conducted through a fluorosilane solution, and finally the wear-resistant and corrosion-resistant hydrophobic titanium alloy surface of the micro-nano structure is obtained. The prepared titanium alloy surface has excellent hardness, wear resistance, film-substrate binding force, hydrophobicity and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of titanium alloys and relates to a method for preparing a wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure. Background Art

[0002] Titanium alloys are widely used in aviation, biomedicine, and mechanical industries due to their excellent properties such as high strength, corrosion resistance, and good biocompatibility. However, in some complex service environments, the shortcomings of poor corrosion resistance and wear resistance still limit their scope of use. For example, titanium alloys used in ship hulls face complex marine working environments with scouring and corrosion, which puts higher requirements on the wear resistance and corrosion resistance of the titanium alloy surface.

[0003] Preparing a ceramic layer on the surface of titanium alloy is an effective method to improve its wear resistance and corrosion resistance. The preparation methods of the surface ceramic layer mainly include spraying, physical vapor deposition, laser cladding, etc. However, it is difficult to prepare a surface ceramic layer with high ceramic volume fraction and high film-base bonding force by the above methods, which restricts the hardness and wear resistance of the titanium alloy surface. At the same time, the poor hydrophobicity of the ceramic layer material limits the further improvement of corrosion resistance. Studies have shown that reducing surface energy and increasing surface roughness are necessary conditions for improving hydrophobicity. Therefore, preparing a micro-nanoscale rough structure on the ceramic layer on the surface of titanium alloy and preparing a hydrophobic material on its surface is a common method to improve corrosion resistance. Methods for preparing a rough surface ceramic layer on the surface of titanium alloy include laser etching, anodizing, chemical / electrochemical etching, template method, sol-gel method, etc. Commonly used hydrophobic film materials include perfluorodecyltriethoxysilane, 1H,1H,2H,2Hperfluorodecyltrihexylsilane, (3,3,3-trifluoropropyl)methyldimethoxysilane, etc.

[0004] However, the current preparation methods of rough surface ceramic layers make it difficult to obtain ceramic layers with both high volume fraction and high membrane-base bonding strength, and the preparation methods of surface rough structures are costly and usually cause a certain degree of damage to the ceramic layer. Therefore, the surface properties are difficult to maintain stably under the action of seawater immersion and scouring, which reduces the wear and corrosion resistance of the surface. Therefore, in order to improve the durability of the corrosion resistance and wear resistance of the titanium alloy surface, it is very necessary to explore new surface treatment methods. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a titanium alloy surface having a micro-nanoscale rough structure and wear resistance, corrosion resistance and hydrophobicity, so as to solve the problem in the prior art that the titanium alloy surface is difficult to have both wear resistance, corrosion resistance and hydrophobicity.

[0006] The technical solution adopted by the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure of the present invention is specifically implemented according to the following steps:

[0007] Step 1, performing surface pretreatment on a titanium alloy, and then preparing micron-sized pits on the surface of the titanium alloy after the surface pretreatment by using a tungsten carbide particle imprinting method;

[0008] Step 2: using a surface treatment process to prepare an iron layer on the surface of the titanium alloy having micron-sized pits to obtain a titanium alloy with an iron layer;

[0009] Step 3, performing high temperature heat treatment on the titanium alloy with the iron layer to form an iron-titanium diffusion layer between the iron layer and the titanium alloy;

[0010] Step 4, carburizing the titanium alloy treated in step 3 to obtain a titanium alloy with an iron layer and a titanium carbide ceramic layer with a micro-nano graded rough structure;

[0011] Step 5, removing the iron layer from the titanium alloy treated in step 4 through a corrosive solution to form a titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure;

[0012] Step 6: prepare a fluorosilane solution with low surface energy, immerse the titanium alloy treated in step 5 in the fluorosilane solution, then take out the immersed titanium alloy and place it in an oven for constant temperature baking, and finally obtain a wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure.

[0013] The present invention is also characterized in that:

[0014] The pretreatment in step 1 is grinding and polishing the surface of the titanium alloy;

[0015] The tungsten carbide particle imprinting method in step 1 is to form micron-sized pits on the surface of the titanium alloy by using spherical tungsten carbide particles under pressure, the pressure range is 60MPa-100MPa;

[0016] In step 2, the surface treatment process is one of physical vapor deposition, chemical vapor deposition, electroplating, and chemical plating;

[0017] The mass fraction of iron in the iron layer in step 2 ranges from 98% to 99.9999%, and the thickness of the iron layer ranges from 1 μm to 30 μm;

[0018] The temperature range of the high temperature heat treatment in step 3 is 800°C-1100°C, and the holding time is 2h-8h;

[0019] In step 4, the carburizing treatment is any one of solid carburizing, gas carburizing, vacuum carburizing and plasma carburizing, the temperature range of the carburizing treatment is 850° C.-1100° C., and the time of the carburizing treatment is 3 h-10 h;

[0020] The corrosion solution in step 5 is specifically a hydrochloric acid solution or a sulfuric acid solution, the mass fraction of hydrochloric acid in the hydrochloric acid solution is 18%-28%, and the mass fraction of sulfuric acid in the sulfuric acid solution is 45%-60%;

[0021] In step 6, the fluorosilane solution is any one of perfluorodecyltriethoxysilane solution, 1H,1H,2H,2H perfluorodecyltrihexylsilane ethanol solution, and (3,3,3 trifluoropropyl)methyldimethoxysilane solution. The concentration of the fluorosilane solution is 0.5wt%-5wt%, the immersion time is 1h-2h, the baking time is 20min-30min, and the oven temperature is 100℃-120℃.

[0022] The beneficial effects of the present invention are:

[0023] (1) The micrometer-scale rough structure is realized by particle imprinting method, which has the advantages of high efficiency, low cost and convenient operation;

[0024] (2) The preparation of nanoscale rough structure is achieved by using the principle of in-situ growth of dendritic TiC in the interdiffusion zone of Ti and Fe elements during carburizing. The surface dendritic TiC has good bonding strength with the titanium carbide layer on the surface of titanium alloy;

[0025] (3) The present invention utilizes carburization to convert the titanium alloy surface into a ceramic layer, so that the ceramic phase is precipitated in situ, the ceramic layer grows inward, and has a high bonding strength with the substrate;

[0026] (4) A micro-nano rough structure composed of titanium carbide is generated on the surface of the titanium alloy, which greatly improves the hydrophobicity of the titanium alloy surface, achieving super hydrophobicity, and effectively improving the wear resistance and corrosion resistance of the titanium alloy surface. It can be applied to special environments and fields and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a preparation flow chart of the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure of the present invention.

[0028] Figure 2 It is a schematic diagram of the titanium alloy surface after carbide particles are embossed in the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure of the present invention.

[0029] Figure 3 It is a schematic diagram of the cross-sectional structure of the titanium alloy after carbide particles are embossed in the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure of the present invention.

[0030] Figure 4 It is a schematic diagram of the cross-sectional structure of the embossed titanium alloy iron plating in the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure of the present invention.

[0031] Figure 5 It is a schematic diagram of the cross-sectional structure of the titanium alloy after heat preservation treatment in the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure of the present invention.

[0032] Figure 6 It is a schematic diagram of the cross-sectional structure of the titanium alloy after carburizing treatment in the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure of the present invention.

[0033] Figure 7 It is a schematic diagram of the cross-sectional structure of the titanium alloy after the iron layer is corroded and removed in the method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure of the present invention. DETAILED DESCRIPTION

[0034] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure of the present invention is specifically implemented according to the following steps:

[0036] Step 1: Take a titanium alloy and perform surface pretreatment, then use a tungsten carbide particle embossing method to form micron-sized pits on the surface of the titanium alloy after surface pretreatment, and obtain a titanium alloy with pits on the surface. Specifically, a PET double-sided tape with a thickness of 10 μm is applied to the surface of the titanium alloy, and a layer of spherical tungsten carbide particles with a particle size of 50 μm-150 μm is attached to the double-sided tape, and a tablet press is used to press at a pressure of 60 MPa-100 MPa. Subsequently, the tungsten carbide particles and PET glue on the surface are washed off with alcohol to obtain a titanium alloy with pits on the surface;

[0037] Step 2, using a surface treatment process to prepare an iron layer on the titanium alloy with pits on the surface, to obtain a titanium alloy with pits and an iron layer on the surface, the surface treatment process is one of physical vapor deposition, chemical vapor deposition, electroplating, and chemical plating, the mass fraction of iron in the iron layer is in the range of 98%-99.9999%, and the thickness of the iron layer is in the range of 1 μm to 30 μm;

[0038] Step 3: Perform high-temperature heat treatment on the titanium alloy with pits and iron layer on the surface, so that the titanium element diffuses into the iron layer. The high-temperature heat treatment temperature ranges from 800°C to 1100°C, and the holding time ranges from 2h to 8h;

[0039] Step 4, carburizing the titanium alloy with pits and iron layer on the surface after high-temperature heat treatment to obtain a titanium alloy with an iron layer and a titanium carbide ceramic layer with a micro-nano graded rough structure; the carburizing temperature range is 850°C-1100°C, the carburizing time range is 3h-10h, preferably, the carburizing method adopts gas carburizing and solid carburizing, and the carburizing treatment temperature range is 950°C-1100°C;

[0040] Step 5: Use a corrosive solution to remove the surface iron layer obtained in step 4, and obtain a titanium carbide ceramic layer with a micro-nano graded rough structure on the surface of the titanium alloy. The corrosive solution is a hydrochloric acid solution and a sulfuric acid solution, the mass fraction of hydrochloric acid in the hydrochloric acid solution is 18%-28%, and the mass fraction of sulfuric acid in the sulfuric acid solution is 45%-60%;

[0041] Step 6: Prepare a fluorosilane solution with low surface energy, immerse the titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure on the surface in the fluorosilane solution for 1h-2h, and then place it in a constant temperature oven for baking for 20min-30min, and the oven temperature range is 100°C-120°C. The fluorosilane solution is one of a perfluorodecyltriethoxysilane solution, a 1H,1H,2H,2H perfluorodecyltrihexylsilane ethanol solution, and a (3,3,3-trifluoropropyl)methyldimethoxysilane solution, and the concentration of the fluorosilane solution is 0.5-5wt%, and the preferred fluorosilane solution is a perfluorodecyltriethoxysilane solution.

[0042] In the present invention, the spherical structure and high hardness of tungsten carbide particles are utilized in step 1, and a single layer of particles is attached to the surface of the titanium alloy by PET double-sided adhesive, and a micron-level rough structure is formed under pressure. During the high-temperature heat treatment process of step 3, titanium and iron elements are fully diffused to form a titanium and iron interdiffusion layer, and titanium elements present a gradient distribution in the iron layer. In the subsequent carburizing process of step 4, in the interdiffusion layer with a titanium element concentration gradient distribution, titanium and carbon react in situ, and titanium carbide with a dendritic micro-nano structure is grown in situ, and the titanium located in the matrix also reacts in situ to form a dense titanium carbide layer, realizing a rough surface with a micro-nano secondary structure. And the iron layer can improve the absorption efficiency of surface active carbon atoms, and prevent oxidation during gas / solid carburizing.

[0043] Embodiment 1:

[0044] This example includes the following steps:

[0045] Step 1: Prepare a Ti6Al4V titanium alloy substrate, pre-treat the titanium alloy surface, and use the tungsten carbide particle embossing method to prepare micron-scale pits on the titanium alloy surface. Specifically, a 10μm thick PET double-sided tape is applied to the titanium alloy sample, and a layer of spherical tungsten carbide particles with a particle size of 50μm is attached to the double-sided tape. Use a tablet press to press for 10 minutes at a pressure of 60MPa. Then use alcohol to clean the tungsten carbide particles and PET glue on the surface;

[0046] Step 2: using magnetron sputtering to prepare an iron layer on the titanium alloy surface with micron-sized pits, wherein the mass fraction of iron in the iron layer is 99.9999% and the thickness of the iron layer is 1 μm;

[0047] Step 3: Perform high-temperature heat treatment on the titanium alloy with pits and iron layer on the surface, so that the titanium element diffuses into the iron layer. The high-temperature heat treatment temperature is 800°C and the holding time is 2 hours;

[0048] Step 4, carburizing the titanium alloy with pits and iron layer on the surface after high-temperature heat treatment, using solid carburizing as the carburizing method, the carburizing temperature is 850°C, and the carburizing time is 3h;

[0049] Step 5, immersing the workpiece obtained in step 4 in a hydrochloric acid solution, and when no bubbles emerge, taking out the workpiece, the iron layer is completely removed, so that the ceramic layer is exposed on the surface, and finally a titanium carbide ceramic layer with a micro-nano graded rough structure is obtained;

[0050] Step 6: prepare a 0.5 wt % perfluorodecyltriethoxysilane solution, immerse the titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure on the surface in the solution for 1 hour, and then bake it in a constant temperature oven at 100° C. for 20 minutes.

[0051] Embodiment 2:

[0052] This example includes the following steps:

[0053] Step 1: Prepare a Ti6Al4V titanium alloy substrate, pre-treat the titanium alloy surface first, and use the tungsten carbide particle embossing method to prepare micron-sized pits on the surface of the titanium alloy after surface pre-treatment. Specifically, a 10μm thick PET double-sided tape is applied to the titanium alloy sample, and a layer of spherical tungsten carbide particles with a particle size of 150μm is attached to the double-sided tape. Use a tablet press to press for 10 minutes under a pressure of 100MPa. Then use alcohol to clean the tungsten carbide particles and PET glue on the surface;

[0054] Step 2: using an electroplating method to prepare an iron layer on the titanium alloy surface having micron-sized pits, wherein the mass fraction of iron in the iron layer is 98% and the thickness of the iron layer is 30 μm;

[0055] Step 3: Perform high temperature heat treatment on the titanium alloy with pits and iron layer on the surface, so that the titanium element diffuses into the iron layer. The high temperature heat treatment temperature is 1100°C and the heat preservation time is 8 hours;

[0056] Step 4: Place the workpiece after high temperature heat treatment in a carburizing furnace and introduce carburizing medium kerosene, toluene, methanol, and ethanol gas for carburizing treatment. The carburizing temperature is 1100°C and the carburizing time is 10 hours;

[0057] Step 5, immersing the workpiece obtained in step 4 in a hydrochloric acid solution, and when no bubbles emerge, taking out the workpiece, the iron layer is completely removed, so that the ceramic layer is exposed on the surface, and finally a titanium carbide ceramic layer with a micro-nano graded rough structure is obtained;

[0058] Step 6: prepare a 5 wt % 1H,1H,2H,2H perfluorodecyltrihexylsilane ethanol solution, immerse the titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure on the surface in the solution for 2 h, and then bake it in a constant temperature oven at 120 ° C for 30 min.

[0059] Embodiment 3:

[0060] This example includes the following steps:

[0061] Step 1: Prepare a Ti substrate, perform surface pretreatment on it, and use the tungsten carbide particle imprinting method to prepare micron-sized pits on the titanium surface after surface pretreatment. Specifically, a 10μm thick PET double-sided tape is applied to the titanium alloy sample, and a layer of spherical tungsten carbide particles with a particle size of 100μm is attached to the double-sided tape. The tablet press is used to press for 10 minutes at a pressure of 80MPa. Then, the tungsten carbide particles and PET glue on the surface are cleaned with alcohol;

[0062] Step 2: using an electroplating method to prepare an iron layer on the titanium alloy surface having micron-sized pits, wherein the mass fraction of iron in the iron layer is 98% and the thickness of the iron layer is 20 μm;

[0063] Step 3: Perform high-temperature heat treatment on the titanium alloy with pits and iron layer on the surface, so that the titanium element diffuses into the iron layer. The high-temperature heat treatment temperature is 950°C and the holding time is 4 hours;

[0064] Step 4, carburizing the titanium alloy with pits and iron layer on the surface after high-temperature heat treatment, using solid carburizing as the carburizing method, the carburizing temperature is 950°C, and the carburizing time is 5h;

[0065] Step 5, immersing the workpiece obtained in step 4 in a hydrochloric acid solution, and when no bubbles emerge, taking out the workpiece, the iron layer is completely removed, so that the ceramic layer is exposed on the surface, and finally a titanium carbide ceramic layer with a micro-nano graded rough structure is obtained;

[0066] Step 6: prepare a 2 wt % perfluorodecyltriethoxysilane solution, immerse the titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure on the surface in the solution for 1.5 h, and then bake it in a constant temperature oven at 110° C. for 25 min.

[0067] Embodiment 4:

[0068] This example includes the following steps:

[0069] Step 1: Prepare a Ti-3Al-2V substrate, pre-treat the titanium alloy surface, and use the tungsten carbide particle embossing method to prepare micron-sized pits on the surface of the titanium alloy after surface pre-treatment. Specifically, a 10μm thick PET double-sided tape is applied to the titanium alloy sample, and a layer of spherical tungsten carbide particles with a particle size of 100μm is attached to the double-sided tape. The tablet press is used to press at a pressure of 80MPa for 10 minutes. Then, the tungsten carbide particles and PET glue on the surface are cleaned with alcohol;

[0070] Step 2: using an electroplating method to prepare an iron layer on the titanium alloy surface having micron-sized pits, wherein the mass fraction of iron in the iron layer is 98% and the thickness of the iron layer is 20 μm;

[0071] Step 3: Perform high-temperature heat treatment on the titanium alloy with pits and iron layer on the surface, so that the titanium element diffuses into the iron layer. The high-temperature heat treatment temperature is 950°C and the holding time is 4 hours;

[0072] Step 4, carburizing the titanium alloy with pits and iron layer on the surface after high-temperature heat treatment, using solid carburizing as the carburizing method, the carburizing temperature is 950°C, and the carburizing time is 5h;

[0073] Step 5, immersing the workpiece obtained in step 4 in a hydrochloric acid solution, and when no bubbles emerge, taking out the workpiece, the iron layer is completely removed, so that the ceramic layer is exposed on the surface, and finally a titanium carbide ceramic layer with a micro-nano graded rough structure is obtained;

[0074] Step 6: prepare a 3 wt % perfluorodecyltriethoxysilane solution, immerse the titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure on the surface in the solution for 2 hours, and then bake it in a constant temperature oven at 120° C. for 30 minutes.

[0075] Embodiment 5:

[0076] This example includes the following steps:

[0077] Step 1: Prepare a Ti-6Al-4V substrate, pre-treat the titanium alloy surface, and use the tungsten carbide particle embossing method to prepare micron-sized pits on the surface of the titanium alloy after surface pre-treatment. Specifically, a 10μm thick PET double-sided tape is applied to the titanium alloy sample, and a layer of spherical tungsten carbide particles with a particle size of 50μm is attached to the double-sided tape. The tablet press is used to press for 10 minutes at a pressure of 60MPa. Then, the tungsten carbide particles and PET glue on the surface are cleaned with alcohol;

[0078] Step 2: using an electroplating method to prepare an iron layer on the titanium alloy surface having micron-sized pits, wherein the mass fraction of iron in the iron layer is 98% and the thickness of the iron layer is 20 μm;

[0079] Step 3: Perform high-temperature heat treatment on the titanium alloy with pits and iron layer on the surface, so that the titanium element diffuses into the iron layer. The high-temperature heat treatment temperature is 1000°C and the holding time is 4 hours;

[0080] Step 4, carburizing the titanium alloy with pits and iron layer on the surface after high temperature heat treatment, using solid carburizing as the carburizing method, the carburizing temperature is 1000°C, and the carburizing time is 5h;

[0081] Step 5, immersing the workpiece obtained in step 4 in a hydrochloric acid solution, and when no bubbles emerge, taking out the workpiece, the iron layer is completely removed, so that the ceramic layer is exposed on the surface, and finally a titanium carbide ceramic layer with a micro-nano graded rough structure is obtained;

[0082] Step 6: prepare a 4 wt % perfluorodecyltriethoxysilane solution, immerse the titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure on the surface in the solution for 2 hours, and then bake it in a constant temperature oven at 120° C. for 20 minutes.

[0083] Performance Test:

[0084] (1) Hardness: The microhardness of the above cases was measured by Vickers microhardness test. The load was 50 g, the indenter was a conical indenter, and the holding time was 10 s.

[0085] (2) Contact angle: The contact angle of the sample surface was measured using a contact angle meter with a droplet volume of 5 μL;

[0086] (3) Salt spray resistance: refer to GB / T17712007, sodium chloride concentration is 60g / L, temperature is 35℃, pH is 7.

[0087] The wear-resistant and hydrophobic titanium alloy surfaces with micro-nano structures prepared in Examples 1-5 were subjected to relevant performance tests, and the test results are shown in the following table:

[0088] project Surface hardness Contact angle (°) Salt spray resistance (60d) Example 1 2300HV 162 No rust Example 2 2550HV 152 No rust Example 3 2450HV 157 No rust Example 4 2400HV 158 No rust Implementation Power 5 2450HV 160 No rust

[0089] The present invention has a method for preparing a wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure to prepare a titanium alloy with a durable super-hydrophobic surface. The micro-nano structure titanium carbide surface hardness obtained by imprinting combined with carburizing can reach an average of 2400HV, and its hardness is greatly improved, and a good wear-resistant effect can be achieved. Tested by a contact angle meter, the water contact angle of the prepared titanium alloy surface is greater than 150°, with excellent hydrophobic properties. And the dense titanium carbide has good corrosion resistance, and no rust phenomenon occurs in the test.

Claims

1. A method for preparing a wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure, characterized in that: Follow the steps below to implement it: Step 1, performing surface pretreatment on a titanium alloy, and then preparing micron-sized pits on the surface of the titanium alloy after the surface pretreatment by using a tungsten carbide particle imprinting method; Step 2: using a surface treatment process to prepare an iron layer on the surface of the titanium alloy having micron-sized pits to obtain a titanium alloy with an iron layer; Step 3, performing high temperature heat treatment on the titanium alloy with the iron layer to form an iron-titanium diffusion layer between the iron layer and the titanium alloy; Step 4, carburizing the titanium alloy treated in step 3 to obtain a titanium alloy with an iron layer and a titanium carbide ceramic layer with a micro-nano graded rough structure; Step 5, removing the iron layer from the titanium alloy treated in step 4 through a corrosive solution to form a titanium alloy having a titanium carbide ceramic layer with a micro-nano graded rough structure; Step 6: prepare a fluorosilane solution with low surface energy, immerse the titanium alloy treated in step 5 in the fluorosilane solution, then take out the immersed titanium alloy and place it in an oven for constant temperature baking, and finally obtain a wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with a micro-nano structure.

2. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: The surface pretreatment in step 1 is grinding and polishing the titanium alloy surface.

3. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: The tungsten carbide particle imprinting method described in step 1 is specifically to apply a PET double-sided tape with a thickness of 10 μm to the surface of the titanium alloy, adhere a layer of spherical tungsten carbide particles with a particle size of 50 μm-150 μm to the double-sided tape, and use a tablet press to press at a pressure of 60 MPa-100 MPa, and then use alcohol to clean off the tungsten carbide particles and PET glue on the surface to obtain a titanium alloy with pits on the surface.

4. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: In step 2, the surface treatment process is one of physical vapor deposition, chemical vapor deposition, electroplating, and chemical plating.

5. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: The mass fraction of iron in the iron layer in step 2 is in the range of 98%-99.9999%, and the thickness of the iron layer is in the range of 1 μm-30 μm.

6. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: The high temperature heat treatment temperature range in step 3 is 800°C-1100°C, and the high temperature heat treatment time is 2h-8h.

7. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: The carburizing treatment in step 3 is any one of solid carburizing, gas carburizing, vacuum carburizing and plasma carburizing. The temperature range of the carburizing treatment is 850° C.-1100° C., and the time of the carburizing treatment is 3 h-10 h.

8. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: The corrosion solution in step 4 is specifically a hydrochloric acid solution or a sulfuric acid solution. The mass fraction of hydrochloric acid in the hydrochloric acid solution is 18%-28%, and the mass fraction of sulfuric acid in the sulfuric acid solution is 45%-60%.

9. The method for preparing the wear-resistant, corrosion-resistant and hydrophobic titanium alloy surface with micro-nano structure according to claim 1, characterized in that: The fluorosilane solution described in step 6 is one of perfluorodecyltriethoxysilane solution, 1H,1H,2H,2H perfluorodecyltrihexylsilane ethanol solution, and (3,3,3-trifluoropropyl)methyldimethoxysilane solution. The concentration of the fluorosilane solution is 0.5wt%-5wt%, the immersion time is 1h-2h, the constant temperature baking time is 20min-30min, and the constant temperature baking temperature range is 100℃-120℃.

Citation Information

Patent Citations

  • Manufacturing method for super hydrophobic surface

    CN103121006A

  • Titanium and titanium alloy surface with hydrophobic and super-hydrophobic characteristics and preparation method thereof

    CN108486633A

  • Titanium alloy surface super-hydrophilic / super-hydrophobic controllable micro-nano composite structure and preparation method thereof

    CN110016658A

  • Preparation method of titanium alloy bionic super-hydrophobic surface

    CN113278958A

  • Treatment method for improving wear-resistant and hydrophobic characteristics of titanium alloy surface

    CN116000313A