Coating preparation method and device

Through the sputtering and high-throughput method of the coating material target on the strip sputtering matrix, the coating of the coating material of the target thickness is determined and prepared, which solves the problem of low coating thickness research efficiency in the prior art and achieves rapid , economical coating performance evaluation.

CN119061369APending Publication Date: 2024-12-03INSTITUTE OF NUCLEAR PHYSICS AND CHEMISTRY CHINA ACADEMY OF ENGINEERING PHYSICS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411186195.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The existing coating preparation methods cannot quickly and efficiently study the impact of coating thickness on coating performance, resulting in large experiment volume and long time consumption, and the choice of thickness in engineering applications is subject to many constraints.

Method used

The long sputtering substrate is sputtered by the coating material target to obtain a coating material coating sample, a thickness range is determined, and a coating material coating of the target thickness is prepared on the target sputtering substrate according to this range, and magnetron sputtering is used to prepare a coating material coating of the target thickness on the target sputtering substrate. The spray technology and high-throughput method study the performance of coatings of different thicknesses.

Benefits of technology

It realizes rapid and efficient study of the impact of coating thickness on performance of coating materials, reduces experimental costs and time, and is suitable for various coatings and thickness-related performance research.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061369A_ABST
    Figure CN119061369A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a coating. The preparation method comprises the following steps: S1, preparing a coating material target; s2, a long-strip-shaped sputtering base body is selected; s3, the long-strip-shaped sputtering base body is sputtered through the coating material target, a coating material coating sample is obtained, and the coating thickness of the coating material on the coating material coating sample is in continuous gradient distribution; s4, determining the thickness range of the coating of the coating material based on the coating sample of the coating material; and S5, based on the thickness range, a coating material coating with the target thickness is prepared on the target sputtering substrate, and a coating product is obtained. A long-strip-shaped sputtering substrate can be sputtered through a coating material target to obtain a coating sample of the coating material, the thickness range of the coating of the coating material is determined according to the coating sample of the coating material, the coating of the coating material with the target thickness is prepared on the target sputtering substrate according to the thickness range, and a coating product is obtained. The problem that an existing coating preparation method cannot rapidly research the influence of the coating thickness of a coating material on the coating performance is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of coating preparation, and in particular to a coating preparation method and device. Background Art

[0002] In research and development and engineering applications, coating thickness is an important indicator and parameter, which is related to the service life and preparation cost of the coating. Traditional coating preparation methods can only prepare coatings of a single thickness at a time. In experimental research and development, determining the optimal thickness of the coating usually requires preparing a series of coatings of different thicknesses. The required amount of experiments is large and time-consuming, which is a huge waste of manpower and material resources. For example, in a nuclear reactor system, an accident-tolerant Cr coating is prepared on the surface of a zirconium alloy, which significantly improves the oxidation resistance of the zirconium alloy matrix and is currently the most widely studied and applied coating. In engineering applications, the thickness of the coating is restricted by many aspects, such as oxidation resistance, neutron economy, etc. However, there is currently a lack of an effective method for quickly and efficiently preparing and screening the thickness of Cr coatings. Summary of the invention

[0003] An embodiment of the present invention provides a coating preparation method, which can be used to sputter a long strip of sputtering substrate through a coating material target to obtain a coating material coating sample, determine the thickness range of the coating material coating based on the coating material coating sample, and prepare a coating material coating of a target thickness on the target sputtering substrate based on the thickness range to obtain a coating product, thereby solving the problem that the existing coating preparation method cannot quickly study the influence of the coating material coating thickness on the coating performance.

[0004] In a first aspect, an embodiment of the present invention provides a coating preparation method, the coating preparation method comprising:

[0005] S1. Prepare coating material target;

[0006] S2, select a long strip sputtering substrate;

[0007] S3, sputtering the long strip sputtering substrate by the coating material target to obtain a coating material coating sample, wherein the coating material coating thickness on the coating material coating sample presents a continuous gradient distribution;

[0008] S4. Determine the thickness range of the coating material based on the coating material sample;

[0009] S5. Based on the thickness range, prepare a coating of a coating material with a target thickness on a target sputtering substrate to obtain a coating product.

[0010] Optionally, the step S2 includes:

[0011] Grinding the long strip sputtering substrate; and

[0012] The long strip sputtering substrate is subjected to a first cleaning treatment, and after the cleaning is completed, it is taken out and dried for later use.

[0013] Optionally, the first cleaning process is performed on the long strip sputtering substrate, and after the cleaning is completed, the long strip sputtering substrate is taken out and dried for standby use, including:

[0014] Performing a first ultrasonic cleaning treatment on the long strip sputtering substrate in acetone; and

[0015] The long strip sputtering substrate is subjected to a second ultrasonic cleaning treatment in alcohol, and after the cleaning is completed, it is taken out and dried for later use.

[0016] Optionally, before step S3, the method further includes:

[0017] The long strip sputtering substrate is subjected to a second cleaning process.

[0018] Optionally, the step S3 includes:

[0019] Placing the coating material target on the target position of the magnetron sputtering equipment;

[0020] Mounting the long strip sputtering substrate on a fixture of the magnetron sputtering device;

[0021] The long strip sputtering substrate is sputtered by adjusting the power of the coating material target and the target position inclination angle to obtain a coating material coating sample.

[0022] Optionally, the step S4 includes:

[0023] Cutting the coating sample of the coating material to obtain a metallographic specimen of the coating material;

[0024] The metallographic sample of the coating of the coating material is screened to determine the thickness range of the coating of the coating material.

[0025] Optionally, the step of cutting the coating material sample to obtain a metallographic specimen of the coating material comprises:

[0026] The coating material sample is subjected to a first cutting process to obtain a plurality of small coating material samples having the same size;

[0027] The small samples of the coating material with the same size are subjected to a steam oxidation experiment to obtain the small samples of the coating material after oxidation;

[0028] The oxidized coating material small sample is subjected to a second cutting process to obtain a metallographic sample of the coating material. In a second aspect, an embodiment of the present invention further provides a coating preparation device, the device comprising:

[0029] A preparation module, used for preparing coating material targets;

[0030] A selection module is used to select a long strip sputtering substrate;

[0031] A sputtering module, used for sputtering the elongated sputtering substrate through the coating material target to obtain a coating material coating sample, wherein the coating material coating thickness in the coating material coating sample presents a continuous gradient distribution;

[0032] A determination module, used to determine the thickness range of the coating of the coating material based on the coating sample of the coating material;

[0033] The preparation module is used to prepare a coating of a coating material with a target thickness on a target sputtering substrate based on the thickness range to obtain a coating product.

[0034] By adopting the coating preparation method of the present invention, a long strip sputtering substrate can be sputtered by a coating material target to obtain a coating material coating sample. According to the coating material coating sample, the thickness range of the coating material coating can be determined, and according to the thickness range, a coating material coating of a target thickness is prepared on the target sputtering substrate to obtain a coating product, thereby solving the problem that the existing coating preparation method cannot quickly study the influence of the coating material coating thickness on the coating performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0036] Figure 1 It is a schematic flow chart of a coating preparation method provided by an embodiment of the present invention;

[0037] Figure 2 It is a schematic structural diagram of target material and substrate installation in a coating preparation method provided by an embodiment of the present invention;

[0038] Figure 3 is a thickness distribution diagram of a coating of a coating material in a coating preparation method provided by an embodiment of the present invention;

[0039] Figure 4 The SEM cross-sectional morphology of coatings of coating materials with different thicknesses after oxidation for different times provided by the embodiments of the present invention;

[0040] Figure 5 It is a model diagram of the anti-oxidation performance of the coating material provided by the embodiment of the present invention - coating thickness - oxidation time;

[0041] Figure 6 It is a structural schematic diagram of a coating preparation device provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] like Figure 1 As shown, Figure 1 1 is a schematic flow chart of a coating preparation method provided by an embodiment of the present invention. The coating preparation method comprises:

[0044] S1. Prepare coating material target.

[0045] In an embodiment of the present invention, the above-mentioned coating material target can be a metal target, such as a pure Cr target, and the size of the target is Φ60mm×5mm. The coating material target can also be other metals, such as iron Fe, nickel Ni and other metals. The second material target can be a non-metal. The above-mentioned coating material target can be any material that can be coated.

[0046] It should be noted that the present invention is specifically described using a pure Cr target as an example.

[0047] S2. Select a long strip sputtering substrate.

[0048] In the embodiment of the present invention, the above-mentioned long strip sputtering substrate can be a metal alloy substrate, for example, a long strip zirconium alloy substrate (Zry-4 alloy substrate), and the size of the long strip zirconium alloy is 145mm×20mm×1.2mm. The above-mentioned long strip sputtering substrate can also be a metal substrate or a long strip ceramic substrate.

[0049] It should be noted that the present invention is specifically described by taking a long strip zirconium alloy substrate as an example.

[0050] Select a long strip of zirconium alloy as a sputtering substrate, use #200--#2000 sandpaper to grind the strip of zirconium alloy substrate, then ultrasonically clean it in acetone and alcohol, and after cleaning, take it out and dry it for use. The cleaning time can be 15 minutes, 16 minutes, 17 minutes, etc., and specifically can be 15 minutes.

[0051] S3. Sputtering the long strip sputtering substrate through the coating material target to obtain a coating material coating sample.

[0052] In an embodiment of the present invention, the thickness of the coating material on the coating material sample presents a continuous gradient distribution.

[0053] The above-mentioned sputtering can be performed by magnetron sputtering technology, or by arc, electron beam and other technologies, and is a process in which a long strip sputtering substrate is sputtered and coated with a coating material target. The above-mentioned magnetron sputtering technology is a physical vapor deposition (PVD) process, which is characterized by low deposition temperature, fast deposition speed, and high and uniform film quality. Magnetron sputtering technology uses a magnetic field to confine electrons near the surface of the target material, thereby generating more plasma on the surface of the target material, and achieving efficient particle deposition through these plasmas. The temperature of the above-mentioned long strip sputtering substrate is 300°C. The above-mentioned sputtering time can specifically be 4 hours.

[0054] The above-mentioned coating material mapping sample can be a Cr coating sample.

[0055] It should be noted that, by using magnetron sputtering technology or arc, electron beam and other technologies, a pure Cr target is used to sputter-coat a long strip of zirconium alloy substrate to obtain a long strip of sputtering substrate with a Cr coating.

[0056] S4. Determine the thickness range of the coating material based on the coating material sample.

[0057] In the embodiment of the present invention, the thickness range of the coating material may be determined according to the coating material sample.

[0058] The present invention is illustrated by taking a Cr coating sample as a coating sample of a coating material.

[0059] The Cr coating samples were cut into 9mm×9mm sizes in the thickness gradient direction of the Cr coating samples, with a total of 16 small Cr coating samples. The thickness of the Cr coating in the small samples of the Cr coating samples was tested by scanning electron microscopy (SEM-EDS); under the same experimental conditions, the 16 small Cr coating samples were subjected to a 1200℃ steam oxidation experiment. After oxidation, the 16 small Cr coating samples were cut, sealed, ground and polished to obtain 16 small Cr coating sample metallographic specimens, which were observed and screened by scanning electron microscopy (SEM-EDS) to determine the thickness range of the Cr coating.

[0060] S5. Based on the thickness range, a coating of a coating material with a target thickness is prepared on a target sputtering substrate to obtain a coating product.

[0061] In the embodiment of the present invention, the critical transition thickness of the Cr coating can be determined according to the thickness range of the Cr coating, and according to the critical transition thickness of the Cr coating, a Cr coating of a target thickness is prepared on a target sputtering substrate to obtain a CrAl coating product.

[0062] In the embodiment of the present invention, the present invention adopts a high-throughput method to prepare coatings of different thicknesses of coating materials, and studies the anti-oxidation properties of coatings of different thicknesses, including but not limited to the study of the thickness and anti-oxidation properties of coating materials, and can be applied to any coating and performance study related to thickness.

[0063] Specifically, the present invention uses a high-throughput method to prepare Cr coatings of different thicknesses and studies the anti-oxidation properties of coatings of different thicknesses, including but not limited to the study of the thickness and anti-oxidation properties of Cr coatings, and can be applied to any coating and thickness-related performance studies.

[0064] In the embodiment of the present invention, S1, a coating material target is prepared; S2, a long strip sputtering substrate is selected; S3, the coating material target is used to sputter the long strip sputtering substrate to obtain a coating material coating sample, and the coating material coating thickness on the coating material coating sample presents a continuous gradient distribution; S4, based on the coating material coating sample, the coating material coating thickness range is determined; S5, based on the thickness range, a coating material coating of a target thickness is prepared on the target sputtering substrate to obtain a coating product. The coating material target can be used to sputter the long strip sputtering substrate to obtain a coating material coating sample, and the coating material coating thickness range is determined according to the coating material coating sample, and the coating material coating of a target thickness is prepared on the target sputtering substrate according to the thickness range to obtain a coating product, which solves the problem that the existing coating preparation method cannot quickly study the influence of the coating material coating thickness on the coating performance.

[0065] Optionally, step S2 includes: grinding the long strip sputtering substrate; and performing a first cleaning process on the long strip sputtering substrate, and taking it out to dry for later use after cleaning.

[0066] In the embodiment of the present invention, the above-mentioned long strip sputtering substrate can be a metal alloy substrate, for example, a long strip zirconium alloy substrate (Zry-4 alloy substrate), and the size of the long strip zirconium alloy is 145mm×20mm×1.2mm. The above-mentioned long strip sputtering substrate can also be a metal substrate or a long strip ceramic substrate.

[0067] It should be noted that the present invention is specifically described by taking a long strip zirconium alloy substrate as an example.

[0068] The above-mentioned grinding process can be understood as a process of removing rust, oil stains, burrs and other impurities on the surface to make the surface smoother.

[0069] The first cleaning process is specifically ultrasonic cleaning, which is a cleaning method that uses the special effect of ultrasonic waves in liquid to clean the surface of an object. Ultrasonic cleaning can effectively improve the cleaning effect and reduce the labor intensity of manual cleaning.

[0070] It should be noted that a long strip of zirconium alloy was selected as a sputtering substrate, and the long strip of zirconium alloy was polished with #200--#2000 sandpaper, and then ultrasonically cleaned. After cleaning, it was taken out and dried for use.

[0071] Optionally, the elongated sputtering substrate is subjected to a first cleaning treatment, and the steps of taking out and drying it after cleaning include: performing a first ultrasonic cleaning treatment on the elongated sputtering substrate in acetone; and performing a second ultrasonic cleaning treatment on the elongated sputtering substrate in alcohol, and taking out and drying it after cleaning.

[0072] In the embodiment of the present invention, the acetone is an organic solution that can effectively remove impurities such as oil, stains, etc. on the surface of the sputtering substrate. When performing ultrasonic cleaning, the sputtering substrate needs to be completely immersed in acetone, and then the impurities on the surface of the sputtering substrate are peeled off by the vibration of the ultrasonic wave, thereby achieving the purpose of cleaning.

[0073] The alcohol is an organic solvent that can further remove acetone and other impurities remaining on the surface of the sputtering substrate. Similarly, the sputtering substrate needs to be completely immersed in the alcohol, and then the impurities on the surface of the sputtering substrate are peeled off through the vibration of the ultrasonic wave, thereby achieving the purpose of cleaning.

[0074] The ultrasonic cleaning time may be 15 minutes, 16 minutes, 17 minutes, etc., and may be specifically 15 minutes.

[0075] It should be noted that the polished long strip of zirconium alloy was ultrasonically cleaned in acetone for 15 minutes and in alcohol for 15 minutes, and after cleaning, it was taken out and dried for later use.

[0076] Optionally, before step S3, the method further includes: performing a second cleaning process on the long strip sputtering substrate.

[0077] In an embodiment of the present invention, the second cleaning process may be glow discharge cleaning, which is a surface cleaning technique that utilizes the phenomenon that gas is broken down and conducts electricity under the action of an electric field. Glow discharge cleaning utilizes a high voltage electric field to generate corona discharge on the surface of a material, excites gas molecules and forms gas ions, thereby generating a complex chemical reaction on the surface of the material, cleaning dirt and oxidation products on the surface of the material. The second cleaning process may also be ion source cleaning or etching cleaning.

[0078] The second cleaning time may be 15 minutes, 16 minutes, 17 minutes, etc., and may be specifically 15 minutes.

[0079] Optionally, step S3 includes: placing a coating material target on a target position of a magnetron sputtering device; installing a long strip sputtering substrate on a fixture of the magnetron sputtering device; and sputtering the long strip sputtering substrate by adjusting the coating material target power and the target position inclination angle to obtain a coating material coating sample.

[0080] In the embodiment of the present invention, the above-mentioned long strip sputtering substrate can be a metal alloy substrate, for example, a long strip zirconium alloy substrate (Zry-4 alloy substrate), and the size of the long strip zirconium alloy is 145mm×20mm×1.2mm. The above-mentioned long strip sputtering substrate can also be a metal substrate or a long strip ceramic substrate.

[0081] It should be noted that the present invention is specifically described by taking a long strip zirconium alloy substrate as an example.

[0082] The above-mentioned target material may be a metal target material, for example, a pure Cr target material, and the size of the target material is Φ60mm×5mm. The target material of the coating material may also be other metals, such as iron Fe, nickel Ni and other metals. The second material target material may be a non-metal. The above-mentioned coating material target material may be any material that can be coated. The present invention is specifically illustrated by a pure Cr target material, and the power of the above-mentioned coating material target material may be a Cr target material power, and the Cr target material power is 200W, the bias voltage is 70V, the gas pressure is 0.5±0.03Pa, and the argon gas flow rate is 30sccm.

[0083] The target position tilt angle may be 40°, and the target position tilt angle is specifically adjusted according to the coating thickness required by the tester.

[0084] It should be noted that the zirconium alloy substrate is mounted on the fixture of the magnetron sputtering equipment, and the Cr target is placed on the target position of the magnetron sputtering equipment, and the target position inclination angle is 40°; by adjusting the target power and the target position inclination angle, the zirconium alloy substrate is sputtered and coated to obtain a coating material coating sample, and the zirconium alloy substrate temperature is 300°C.

[0085] like Figure 2 As shown, Figure 2It is a structural schematic diagram of the target material and substrate installation of the coating preparation method provided in an embodiment of the present invention. Specifically, the zirconium alloy substrate is installed on the fixture of the magnetron sputtering equipment, and the Cr target is placed on the target position of the magnetron sputtering equipment, and the target position is tilted at 40°; by adjusting the target power and the target position tilt angle, the zirconium alloy substrate is sputtered and coated to obtain a uniform Cr coating. Among them, before the zirconium alloy substrate is installed, it is polished with #200--#2000 sandpaper, then ultrasonically cleaned in acetone and alcohol for 15 minutes each, taken out and dried for use. Before sputtering the zirconium alloy substrate, the zirconium alloy substrate is first glow discharged and cleaned for 15 minutes. The temperature of the zirconium alloy substrate is 300°C. The size of the Cr target is Φ60mm×5mm. The Cr target power is 200W, the bias voltage is 70V, the gas pressure is 0.5±0.03Pa, and the argon gas flow rate is 30sccm. The sputtering time is 4h.

[0086] Optionally, step S4 includes: cutting the coating sample of the coating material to obtain a metallographic sample of the coating material; screening the metallographic sample of the coating material to determine the thickness range of the coating material.

[0087] In the embodiment of the present invention, the above-mentioned cutting process can be understood as a cutting process of cutting the coating material sample into smaller alloy samples along a specific direction and depth using a cutting tool (such as a saw, laser, etc.).

[0088] Scanning electron microscope (SEM) can be used to screen and process the metallographic samples of the coating material to determine the thickness range of the coating material. The above-mentioned scanning electron microscope is an imaging device that can produce high resolution, high magnification and high contrast, and can be used to observe the surface morphology and structural characteristics of the material. Through SEM testing, the thickness range of the coating material can be obtained, and the coating material thickness presents a continuous gradient distribution.

[0089] During the SEM test, the samples were observed using a scanning electron microscope (SEM). The cross-sectional morphology of the zirconium alloy substrate was observed using SEM, and the thickness range of the coating material was determined by analyzing the oxidation condition, thereby determining the critical transition thickness of the coating material.

[0090] Optionally, the step of cutting the coating material sample to obtain a metallographic specimen of the coating material includes: performing a first cutting process on the coating material sample to obtain a plurality of small coating material samples of the same size; performing a steam oxidation experiment on each of the small coating material samples of the same size to obtain oxidized small coating material samples; and performing a second cutting process on the oxidized small coating material samples to obtain a metallographic specimen of the coating material.

[0091] In an embodiment of the present invention, the coating sample of the coating material can be cut into a size of 9mm×9mm along the direction of the sample thickness gradient, with a total of 16 small coating material samples; SEM is used to test the thickness range of the coating material in the 16 small coating material samples.

[0092] Under the same experimental conditions, the steam oxidation experiment can be carried out on small samples of the same size of the coating material coating by the oxidation device pre-set by the system. The above oxidation device can test the oxidation resistance of the coating material coating. The oxidation device can oxidize the sputtered substrate of the prepared coating material coating at one time.

[0093] The temperature of the above steam oxidation experiment is 1200°C.

[0094] The second cutting process can be understood as the process of cutting, sealing, grinding, polishing and other processes. The above-mentioned cutting can be understood as the process of cutting a small sample of the oxidized coating material; the above-mentioned sealing can be understood as the need to seal the cut small sample of the coating material, usually using resin or other materials to seal the cut surface of the sample to prevent it from being damaged during subsequent processing; the above-mentioned grinding can be understood as the need to grind the sealed sample to remove the sawtooth marks on the cut surface and make the surface smooth. #200--#2000 sandpaper can be used for grinding during the grinding process. The above-mentioned polishing can be understood as polishing the small sample of the coating material after grinding to achieve a mirror effect on the surface.

[0095] like Figure 3 As shown, Figure 3 is a thickness distribution diagram of a coating material coating in a coating preparation method provided by an embodiment of the present invention. Specifically, Figure 3 As shown in a, after the sputtering coating is completed, the coating material sample is taken out and cut into 9mm×9mm size according to the thickness gradient direction. A total of 16 small coating material samples are obtained. The thickness range of the coating in the small coating material samples is tested by SEM. The thickness distribution is shown in Figure 3 As shown in b, the coating thickness of the coating material presents a continuous gradient distribution, and the coating thickness of the coating material ranges from 3.2 to 16.2 μm.

[0096] Figure 4 The SEM cross-sectional morphology of coatings of different thicknesses after oxidation for different times provided by the embodiments of the present invention. Specifically, the oxidation resistance of coatings of different thicknesses is tested, and a small sample of the coating is subjected to a 1200°C steam oxidation experiment. After oxidation, the small sample of the coating is cut, sealed, ground, and polished to obtain a metallographic sample of the coating. The sample is observed using a scanning electron microscope (SEM), and the SEM cross-sectional morphology of coatings of different thicknesses after oxidation for different times can be obtained. Figure 4 As shown in a, it is the SEM cross-sectional morphology of the coating material after oxidation for 10 minutes. Figure 4 As shown in b, it is the SEM cross-sectional morphology of the coating material after oxidation for 30 minutes. Figure 4 c is the SEM cross-sectional morphology of the coating material after oxidation for 50 minutes. The coating material coating of the present invention is illustrated by taking a Cr coating as an example.

[0097] Figure 5 This is a model diagram of the anti-oxidation performance of the coating material coating-coating thickness-oxidation time provided by the embodiment of the present invention. Specifically, the SEM cross-sectional morphology of the coating material coatings of different thicknesses after oxidation for different times can be used to screen the critical transition thickness of the coating material coating from the oxidation condition of the sputtered substrate, and the model between the anti-oxidation performance of the coating material coating and the thickness of the coating material coating can be obtained by fitting. Figure 5 As shown, the partial protective chromium thickness is configured as y=5.09+0.11x R2=0.999, and the protective chromium thickness is configured as y=2.53*x^0.47R2=0.986. The above critical transition thickness can be understood as the optimal thickness of the coating.

[0098] In the embodiment of the present invention, the present invention uses a pure Cr target material to prepare a Cr coating with a continuous thickness gradient on a long strip zirconium alloy substrate through magnetron sputtering technology, and combines a high-throughput oxidation test method to efficiently and accurately study the corresponding relationship between coating thickness and performance. The present invention can solve the problem that the existing coating preparation method cannot quickly study the influence of the coating thickness of the coating material on the coating performance. The present invention can be applied to any coating and performance research related to thickness.

[0099] like Figure 6 As shown, Figure 6 1 is a schematic diagram of a coating preparation device provided by an embodiment of the present invention. The coating preparation device comprises:

[0100] Preparation module 601, used for preparing coating material target;

[0101] A selection module 602 is used to select a long strip sputtering substrate;

[0102] A sputtering module 603 is used to sputter the long strip sputtering substrate through the coating material target to obtain a coating material coating sample, wherein the coating material coating thickness on the coating material coating sample presents a continuous gradient distribution;

[0103] A determination module 604 is used to determine the thickness range of the coating material based on the technical coating sample;

[0104] The preparation module 605 is used to prepare a coating of a coating material with a target thickness on a target sputtering substrate based on the thickness range to obtain a coating product.

[0105] Optionally, the step S2 is also used to perform a grinding process on the elongated sputtering substrate; and perform a first cleaning process on the elongated sputtering substrate, and after cleaning, take it out and dry it for later use.

[0106] Optionally, the step S2 is also used to perform a first ultrasonic cleaning treatment on the long strip sputtering substrate in acetone; and perform a second ultrasonic cleaning treatment on the long strip sputtering substrate in alcohol, and after cleaning, take it out and dry it for later use.

[0107] Optionally, the device further comprises:

[0108] The cleaning module is used for performing a second cleaning process on the long strip sputtering substrate.

[0109] Optionally, the step S3 is also used to place the coating material target on the target position of the magnetron sputtering equipment; install the elongated sputtering substrate on the fixture of the magnetron sputtering equipment; and sputter the elongated sputtering substrate by adjusting the coating material target power and the target position inclination angle to obtain a coating material coating sample.

[0110] Optionally, the step S4 is also used to cut the coating material sample to obtain a metallographic sample of the coating material; and screen the coating material metallographic sample to determine the thickness range of the coating material.

[0111] Optionally, the step S4 is also used to perform a first cutting process on the coating material sample to obtain a plurality of small coating material samples of the same size; perform a steam oxidation experiment on each of the small coating material samples of the same size to obtain an oxidized small coating material sample; perform a second cutting process on the oxidized small coating material sample to obtain a metallographic specimen of the coating material sample.

[0112] The coating preparation device provided in the embodiment of the present invention can realize each process realized by the coating preparation method in the above method embodiment and can achieve the same beneficial effects. To avoid repetition, it will not be described here.

[0113] The above disclosure is only the preferred embodiment of the present invention, which certainly cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.

Claims

1. A coating preparation method, characterized in that: The coating preparation method comprises: S1. Prepare coating material target; S2, select a long strip sputtering substrate; S3, sputtering the long strip sputtering substrate by the coating material target to obtain a coating material coating sample, wherein the coating material coating thickness on the coating material coating sample presents a continuous gradient distribution; S4. Determine the thickness range of the coating material based on the technical coating sample; S5. Based on the thickness range, prepare a coating of a coating material of a target thickness on a target sputtering substrate to obtain a coating material coating product.

2. The coating preparation method according to claim 1, characterized in that: The step S2 comprises: Grinding the long strip sputtering substrate; and The long strip sputtering substrate is subjected to a first cleaning treatment, and after the cleaning is completed, it is taken out and dried for later use.

3. The coating preparation method according to claim 2, characterized in that: The first cleaning process is performed on the long strip sputtering substrate, and after the cleaning is completed, the long strip sputtering substrate is taken out and dried for standby use, comprising: Performing a first ultrasonic cleaning treatment on the long strip sputtering substrate in acetone; and The long strip sputtering substrate is subjected to a second ultrasonic cleaning treatment in alcohol, and after the cleaning is completed, it is taken out and dried for later use.

4. The coating preparation method according to claim 3, characterized in that: Before step S3, the method further includes: The long strip sputtering substrate is subjected to a second cleaning process.

5. The coating preparation method according to claim 4, characterized in that: The step S3 comprises: Placing the coating material target on the target position of the magnetron sputtering equipment; Mounting the long strip sputtering substrate on a fixture of the magnetron sputtering device; The long strip sputtering substrate is sputtered by adjusting the power of the coating material target and the target position inclination angle to obtain a coating material coating sample.

6. The coating preparation method according to claim 5, characterized in that: The step S4 comprises: Cutting the coating sample of the coating material to obtain a metallographic specimen of the coating material; The metallographic sample of the coating of the coating material is screened to determine the thickness range of the coating of the coating material.

7. The coating preparation method according to claim 6, characterized in that: The step of cutting the coating material sample to obtain a metallographic specimen of the coating material comprises: The coating material sample is subjected to a first cutting process to obtain a plurality of small coating material samples having the same size; The small samples of the coating material with the same size are subjected to a steam oxidation experiment to obtain the small samples of the coating material after oxidation; The oxidized small sample of the coating material is subjected to a second cutting process to obtain a metallographic sample of the coating material.

8. A coating preparation device, characterized in that: The device comprises: A preparation module, used for preparing coating material targets; A selection module is used to select a long strip sputtering substrate; A sputtering module, used for sputtering the elongated sputtering substrate through the coating material target to obtain a coating material coating sample, wherein the coating material coating thickness in the coating material coating sample presents a continuous gradient distribution; A determination module, used to determine the thickness range of the coating of the coating material based on the coating sample of the coating material; The preparation module is used to prepare a coating of a coating material with a target thickness on a target sputtering substrate based on the thickness range to obtain a coating product.

Citation Information

Patent Citations

  • Method for preparing high-throughput Co-Al-W based alloy thin film with magnetron sputtering technology

    CN109306461A

  • Titanium alloy continuous gradient high-temperature-resisting coating and preparation method thereof

    CN110076340A

  • High flux method for efficiently screening out growth conditions of high-quality carbon nanotubes

    CN110592556A

  • High-flux thickness gradient film and preparation method thereof

    CN116121704A

  • Magnetic element and its manufacturing method and its manufacturing apparatus

    JP1998116715A