Construction process of sodium-philic alloying interface and sodium metal battery prepared from sodium-philic alloying interface
By constructing a sodium-philic alloying interface on the negative electrode surface of the sodium metal battery and matching it with the Prussian blue analog, the problem of sodium dendrites is solved, the cycle life and electrochemical performance of sodium metal battery are improved, and high energy density and safety performance are achieved Improvement.
Patent Information
- Application Number
- CN202411549936.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-01
- Publication Date
- 2024-12-03
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Sodium dendrites are prone to grow on the negative electrode side of sodium metal batteries, resulting in safety problems and short cycle life, hindering its commercialization process.
Using the construction method of sodium-philic alloying interface, by uniformly applying metal powders such as Bi, Sn, etc. to the surface of the sodium metal negative electrode, the alloy frame is formed through the accumulation roller bonding technology to guide sodium metal nucleation, reduce the nucleation overpotential, and inhibit the Dentites are generated and matched with Prussian blue analogs as a positive electrode material to improve rate performance and cycle stability.
Effectively inhibit the formation of sodium dendrites, improve the cycle life and electrochemical performance of sodium metal batteries, enhance the stability of the negative electrode structure and the Coulomb efficiency, reduce the consumption and decomposition of the electrolyte, and achieve high energy density and safety performance. Improvement.
Smart Images

Figure CN119061392A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries, and in particular relates to a process for constructing a sodium-philic alloying interface and a sodium metal battery prepared therefrom. Background Art
[0002] The reserves of fossil fuels (oil, coal, and natural gas, etc.) are limited and will cause serious pollution to the environment. In order to meet the development needs of human society, the development of efficient, clean, and renewable new energy has become one of the most concerned hot topics in today's society. Nowadays, lithium-ion batteries have been studied by many researchers because of their own advantages, such as high specific energy, working voltage, and very good cycle performance. They have been widely used in new energy vehicles and small mobile devices. For example, wind farms, solar power stations and other new energy power generation equipment are usually equipped with corresponding energy storage devices to improve energy utilization efficiency. New energy vehicles will use lithium-ion batteries instead of fuel engines as a power source, and portable mobile devices will also use lithium batteries as an energy source, which also increases our demand for lithium (Li) resources. However, the availability of lithium is very limited, and the storage capacity of lithium in the earth's crust is only 0.0017%.
[0003] Sodium reserves are more abundant, and sodium-ion batteries have similar electrochemical properties to lithium-ion batteries. They follow the working principle of "rocking chair batteries" and are expected to become a substitute for lithium-ion batteries. The structure and working principle of sodium-ion batteries are similar to those of lithium-ion batteries. They are composed of four main parts: positive electrode, negative electrode, diaphragm, and electrolyte. The negative electrode materials of sodium-ion batteries include carbon-based materials (graphene, graphite, hard carbon, etc.) and titanium-based oxides (titanium dioxide, sodium titanate, etc.). Conversion materials include transition metal oxide-based materials (iron oxide, cobalt oxide, copper oxide, etc.), transition metal sulfide-based materials (molybdenum sulfide, tin sulfide, etc.) and transition metal phosphides (nickel phosphide, etc.). Alloying reaction materials include alloy compounds (sodium germanium alloy, sodium antimony alloy, etc.). Among these sodium-ion battery negative electrode materials, the sodium metal negative electrode has a high theoretical specific capacity (about 1166 mAh g -1 ), low redox potential (about -2.71 V, compared to the standard hydrogen electrode potential) is considered to be the most promising negative electrode material. However, the application of metallic sodium negative electrode faces great challenges, because it will have severe dendrite growth and severe side reactions with the electrolyte during charging, which often leads to safety issues and short cycle life. The above reasons have seriously hindered the commercialization of sodium metal negative electrode, and it has not yet been mass-produced and applied.
[0004] Therefore, in order to achieve sodium metal batteries with high energy density and high safety performance, we must focus on solving and eradicating the problem of sodium dendrite growth and optimizing interface stability, which is also the key to achieving the safety and long life of sodium metal batteries. Summary of the invention
[0005] The purpose of the present invention is to solve the problem that sodium dendrites are easily grown on the negative electrode side of the existing sodium metal battery, and a construction and preparation method of a sodium-philic alloying interface and a practical application of a sodium metal full battery matching with a positive electrode material are proposed. The constructed sodium-philic alloying interface has an alloy skeleton, which can effectively guide the nucleation of sodium metal during the battery cycle, reduce the nucleation overpotential, inhibit the formation of sodium dendrites, reduce the current density of the electrochemical reaction, inhibit volume expansion, and improve the cycle life of the battery. In addition, the sodium-philic alloying interface provides sodium-philic sites, which is conducive to the nucleation and uniform deposition of the sodium metal battery, and improves the coulombic efficiency. After the sodium-philic alloying interface is constructed, it is used as a sodium metal negative electrode, and a Prussian blue analogue is used as a positive electrode, which improves its rate performance and inhibits the consumption and decomposition of the electrolyte, providing a new idea for solving the problem that the existing sodium metal negative electrode is prone to the growth of uncontrollable sodium dendrites, resulting in a decrease in cycle life.
[0006] In order to solve the above-mentioned problems of some sodium metal batteries and achieve the above-mentioned objectives, the technical solution adopted by the present invention is: The present invention provides a construction and preparation method of a sodium-philic alloying interface, comprising the following steps: First, the sodium block is shaved into smooth sodium blocks in a glove box, and then repeatedly rolled by mechanical methods to obtain thinner sodium metal sheets.
[0007] The powder is evenly applied on the surface of the sodium sheet. Through the cumulative roller bonding technology, the color change of the surface of the sodium metal sheet can be clearly seen. The powder is one or two of Zn, Bi, Sn, Fe, Cu, Ti, Mg, SnF2, SnCl3, SnBr3, BiF3, BiCl3, and BiBr3.
[0008] The sodium-philic alloying interface constructed in the present invention can effectively guide the nucleation of sodium metal, reduce the nucleation overpotential, and inhibit the formation of sodium dendrites. Metals such as Bi and Sn can effectively reduce the nucleation sites of sodium, so that it is uniformly deposited on the surface of sodium metal. In addition, sodium metal with a sodium-philic alloying interface is used as a negative electrode, and the synthesized Prussian blue analogue is used as a positive electrode material to match the sodium metal battery, which can effectively improve the rate performance and cycle at a high current density, and can inhibit the decomposition of the electrolyte. Since sodium metal forms a sodium-philic alloying interface with a metal element or a metal compound, the growth of dendrites is inhibited, and it is a more ideal sodium metal negative electrode.
[0009] The preparation method of the present invention is simple to operate. A sodium-affinity alloying interface is constructed by a cumulative rolling bonding method at room temperature. The sodium alloy phase and a phase mixed with sodium metal constitute an alloy skeleton, which can improve sodium affinity, facilitate sodium ion transport, improve the stability of the negative electrode structure, and inhibit the consumption and decomposition of the electrolyte. The electrochemical performance of the sodium battery is improved through the joint action of the alloy skeleton.
[0010] Preferably, the protective gas of the glove box is argon or nitrogen.
[0011] Preferably, the thickness of the sodium metal flakes is 250 um.
[0012] Preferably, the mass percentage of the metal powder is 1%.
[0013] Preferably, the thickness of the sodium metal alloy composite material after rolling after the powder is added is 200 um.
[0014] Preferably, the rolling time is 20-30 min.
[0015] The second aspect of the present invention provides a sodium metal battery, the sodium metal battery comprising a positive electrode, a negative electrode and an electrolyte; the negative electrode is the sodium metal negative electrode containing a sodium-philic alloying interface. The positive electrode is a Prussian blue analog synthesized by coprecipitation, contains fewer defects, and has a simple method and process, simple equipment, and widely available raw materials, and has better performance.
[0016] Preferably, the sodium salt of the electrolyte is sodium perchlorate, the solvent is propylene carbonate, and the concentration of the sodium perchlorate is 1-2 mol.
[0017] Preferably, the structure of the sodium metal battery further comprises a separator, and the separator is Whatman glass fiber, cellulose separator, or PP separator.
[0018] Compared with the prior art, the advantages of the present invention are: In the present invention, the sodium metal negative electrode of the sodium-philic alloying interface is formed into a thin sheet by cumulative rolling of sodium metal and other metal element powders or metal compound powders at room temperature, thereby obtaining a sodium alloy phase and some non-sodium phase materials. The changes on the surface of the sodium metal can be seen during the rolling process, and the formed alloy skeleton can guide the uniform deposition of the sodium metal battery during the cycle process, reduce the formation of sodium dendrites and the deposition of dead sodium, improve the cycle stability of the battery, and accelerate the transmission of sodium ions. In addition, the operation is simple, which is conducive to industrial large-scale production, and solves the problem that the growth of sodium negative electrode side dendrites is uncontrollable and the cycle performance of sodium metal batteries is reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1It is the SEM image of the Prussian blue analogue positive electrode material.
[0020] Figure 2 a, b, c, d, e, and f are comparison diagrams of the metal sodium alloy negative electrodes of Comparative Example 1, Comparative Example 2, Example 3, Example 4, Example 6, and Example 7, respectively.
[0021] Figure 3 This is the XRD comparison chart of metallic sodium anode, commercial Bi and Bi@Na.
[0022] Figure 4 It is a comparison chart of battery impedance at room temperature in Example 3, Example 4 and Comparative Example 1.
[0023] Figure 5 The cells of Example 1 and Example 3 were compared at 0.5 mA cm -2 Comparison diagram under current density.
[0024] Figure 6 The comparison of the batteries in Example 1 and Example 2 shows that the -2 Comparison diagram under current density.
[0025] Figure 7 The results are shown in Table 1. The results are shown in Table 1. The results are shown in Table 1. -2 Comparison diagram under current density.
[0026] Figure 8 This is a comparison of the overpotentials of asymmetric sodium batteries formed by several different metals and Cu foil.
[0027] Fig. 9 a and b are the dendrite observation images of the full battery matched with Prussian blue in Comparative Example 1.
[0028] Fig.10 a and b are the dendrite observation images of the full battery matched with Prussian blue in Example 3.
[0029] Fig.11 It is a comparison chart of the rate performance of the full battery matched with Prussian blue in Example 3 and Comparative Example 1.
[0030] Fig.12 The current density of the full battery matched with Prussian blue in Example 3 and Comparative Example 1 is 1000 mA g -1 Comparison of the first cycle charge and discharge curves.
[0031] Fig.13 Current density of full cell after matching with Prussian blue in Example 3 and Comparative Example 1 is 1000 mA g -1 The comparison chart after 300 cycles.
[0032] Fig.14 The current density of the full battery after matching with Prussian blue in Example 3 and Comparative Example 1 is 1000 mA g -1 Comparison picture of the diaphragm being disassembled after 300 cycles.
[0033] Fig.15 The current density of the full battery matched with Prussian blue in Example 4 and Comparative Example 1 is 100 mAg -1 Comparison of the first cycle charge and discharge curves.
[0034] Fig.16 The current density of the full cell after matching the Prussian blue of Example 4 and Comparative Example 1 is 100 mA g -1 Comparison chart after 500 cycles.
[0035] Fig.17 The current density of the full battery matched with Prussian blue in Example 5 and Comparative Example 1 is 100 mAg -1 Comparison of the first cycle charge and discharge curves. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Example
[0037] Preparation of Prussian blue analogue cathode materials Ferrous sulfate (4 mmol) and manganese sulfate (1 mmol) were dissolved in 100 ml of deionized water and stirred for 3 h, which was recorded as solution A. Sodium ferrocyanide (5 mmol) was dissolved in 100 ml of deionized water and stirred for 3 h, which was recorded as solution B. Solution A and solution B were simultaneously dripped into solution C (50 ml of deionized water was added to solution C) at a rate of 20 ml / h, and aged for 24 h after the dripping was completed. The lower precipitate was then washed with water and ethanol, and the material was freeze-dried in a freeze dryer for 12 h and then collected to obtain an iron-manganese-based Prussian blue analogue containing crystal water and defects (referred to as FeMn-PBA) Example
[0038] Preparation of positive electrode The positive electrode was prepared by mixing the FeMn-PBA material, conductive carbon black (conductive agent) and sodium alginate (binder) in Example 1 in a ratio of 80:10:10 (wt%) in a shaking tube, adding 6 3 mm zirconium dioxide particles, shaking thoroughly, and applying the resulting uniform slurry evenly on an aluminum foil (current collector) through a coating machine, and placing it at 100 oC was dried in a vacuum drying oven for 12 h to completely evaporate the solvent, and then cut into circular electrodes with a diameter of 10 mm using a cutting machine. The electrodes were weighed and the mass of the active substance was calculated to be ~2.5 mg. Example
[0039] At present, sodium metal batteries all have a common problem, that is, uncontrollable sodium dendrite growth. Sodium metal negative electrodes without any modification are prone to the growth of sodium dendrites and are prone to overcharging. The sodium metal negative electrode with a sodium-affinity alloying interface constructed in Example 3 is a sodium metal negative electrode obtained by evenly applying metal powder on the surface of sodium metal and cumulatively rolling it. The sodium alloy phase and the phase mixed with sodium metal constitute an alloy skeleton, which can improve sodium affinity, facilitate sodium ion transport, improve the stability of the negative electrode structure, and inhibit the consumption and decomposition of the electrolyte. The electrochemical performance of the sodium battery is improved through the joint action of the alloy skeleton. It also improves the rate performance of the sodium metal battery (electrode plate with Prussian blue as the positive electrode) and enhances its diffusion coefficient during discharge. The steps included are as follows: First, use a rolling machine to roll the bulk sodium metal into thin sheets (thickness is about 100 um).
[0040] Metal bismuth (Bi) powder was evenly sprinkled on the surface of sodium metal flakes, where the mass ratio of Bi to Na was 1:100. After uniform mixing, it was cut into discs (denoted as Bi@Na). The above operations were completed in an argon glove box (0wt%≤0.01, H2O wt%≤0.01).
[0041] The Bi@Na in step (2) was assembled into a pair of batteries, where the electrolyte used in the sodium metal battery was a solution of NaClO4 dissolved in ethyl methyl carbonate and propylene carbonate (volume ratio 1:1) and 5 wt% fluoroethylene carbonate additive, where the concentration of NaClO4 was 1 mol / L; the separator was a glass fiber membrane (produced by Whatman). The current density of the battery test was 0.5 mA cm -2 .
[0042] The positive electrode prepared in Example 2 is matched to a sodium metal battery. The electrolyte has the same formula as that in step (3). The test voltage window is 2-4.0 V and the current density is 1000 mA g -1 .
[0043] Battery assembly conditions: All battery assemblies were completed in a glove box (0 wt%≤0.01, H2O wt%≤0.01). Constant current charge-discharge test and long cycle test of R2032 button cell were achieved by Neware CT4000. Example
[0044] The difference between this embodiment and the third embodiment is that the metal bismuth (Bi) is replaced with the metal tin (Sn) with the same content, and the rest is the same as the third embodiment. Example
[0045] The difference between this embodiment and embodiment 3 is that the metal bismuth (Bi) is replaced with the metal tin (Zn) of the same content, and the rest is the same as embodiment 3. Example
[0046] The difference between this embodiment and embodiment 3 is that metal bismuth (Bi) is replaced with metal iron (SnF2) of the same content, and the rest is the same as embodiment 3. Example
[0047] The difference between this embodiment and embodiment 3 is that metal bismuth (Bi) is replaced with bismuth fluoride powder (BiF3) of the same content, and the rest is the same as embodiment 3. Example
[0048] The difference between this embodiment and embodiment 3 is that metal bismuth (Bi) is replaced with bismuth chloride powder (BiCl3) of the same content, and the rest is the same as embodiment 3.
[0049] Comparative Example 1 This comparative example provides a sodium metal negative electrode that has not been modified. Other steps (1), (3), (4), and (5) are the same as those in Example 3.
[0050] Comparative Example 2 The difference between this comparative example and Example 3 is that metal bismuth (Bi) is replaced with metal iron (Fe) of the same content, and the rest is the same as Example 3.
[0051] Figure 1 This is the SEM of the Prussian blue analogue positive electrode material in Example 1. It can be seen that the morphology of the material is regular and in the shape of a cubic block.
[0052] Figure 2 a, b, c, d, e, and f are comparison diagrams of the metal sodium alloy negative electrodes of Comparative Example 1, Comparative Example 2, Example 3, Example 4, Example 6, and Example 7, respectively. It can be seen that there is a very obvious color change on the surface of Na metal and Fe, Bi, Sn, SnF2, and BiF3 powders at room temperature, that is, an alloy is generated on the surface.
[0053] Figure 3 This is a comparison chart of XRD of Example 3, Comparative Example 1 and commercial metal Bi. It can be seen that there are Na and Bi phases in the XRD, which can prove that an alloy is produced.
[0054] Figure 4From the comparison diagram of the battery impedance at room temperature in Example 3, Example 4 and Comparative Example 1, it can be seen that the impedance of the sodium metal negative electrode decreases after the sodium-philic alloying interface is constructed, the impedance of the Bi@Na alloy negative electrode is the smallest, which is 56.8Ω, followed by the Sn@Na alloy negative electrode, which is 145.8Ω, and the impedance of Comparative Example 1 without the sodium-philic alloying interface is the largest, which is 240.3Ω. Therefore, the formation of the interface layer effectively reduces the internal resistance of the battery, thereby improving the rate performance of the battery.
[0055] Figure 5 The symmetrical battery 0.5 mAh cm of Example 3 and Comparative Example 1 -2 From the comparison chart under current density, it can be seen that the modified Bi@Na alloy negative electrode has reduced its overpotential and the cycle life in ester organic electrolyte has reached 500h.
[0056] Figure 6 The comparison example and the comparison example 2 are for the battery 0.5 mAh cm -2 From the comparison diagram under current density, it can be seen that Fe metal, which only has a composite effect with Na metal, fails to change the tip of the first circle and the polarization of the first circle, but also enhances its cycle life. However, the improvement effect is not as good as the effect of Bi and Na forming an alloy.
[0057] Figure 7 The battery of Example 4 and Comparative Example 1 and Comparative Example 2 is 0.5 mAh·cm -2 From the comparison chart under current density, Sn metal and Na metal can form alloys at room temperature. It can be seen that the cycle life of the battery is longer than that of the negative electrode assembly of Fe and Na composite, but it is longer than the cycle life of pure sodium metal. This also proves that some metals forming alloys with Na or not forming alloys are beneficial to increase their cycle life.
[0058] Figure 8 It is a comparison chart of the overpotentials of Example 3 and Example 4 as well as Comparative Examples 1 and 2. It can be seen that the overpotential of the Bi@Na alloy negative electrode is the lowest, which is 42 mV, and the overpotential of Sn@Na is also lower than that of sodium metal.
[0059] Fig. 9 a, b are the dendrite observation pictures of the full battery matched with Prussian blue in Comparative Example 1. It can be seen that in the comparison between the initial and the time when charged to 4 V, the dendrites grow a lot and irregularly.
[0060] Fig.10 a, b are the dendrite observation images of the full battery matched with Prussian blue in Example 3. It can be seen that the comparison between the initial and the time when charged to 4 V shows that after the sodium-philic alloying interface is constructed, the growth of dendrites is suppressed after the sodium metal negative electrode and the positive electrode are matched into a metal battery.
[0061] Fig.11 The rate performance comparison of the full battery in Example 3 and Comparative Example 1 shows that the current density of Bi@Na||PB is 4000 mAh g -1 When the specific capacity is 100 mAh g -1 , while Na||PB is 4000 mAh g -1 Specific capacity remaining 60mAh g -1 , so the modified Na metal can improve the rate performance of Prussian blue analog materials.
[0062] Fig.12 Example 3 matches Comparative Example 1 and the current density is 1000 mAh g -1 From the comparison of the first-cycle curves, it can be seen that the unmodified sodium metal cathode has a voltage drop during the discharge process, while after modification with Bi metal, there is a significant improvement and its polarization is reduced.
[0063] Fig.13 Example 3 is matched with Comparative Example 1 and the current density is 1000 mA g -1 The comparison chart after 300 cycles shows that during the fast charging process, the capacity retention rate of Bi@Na||PB after 300 cycles is 77.64%, and the remaining capacity is 108.55 mAh g-1. The capacity retention rate of Na||PB after 300 cycles is 45.73%, and the remaining capacity is 64.12 mAh g-1. -1 This is because the alloy formed by the Bi@Na negative electrode can reduce the consumption and decomposition of the electrolyte.
[0064] Fig.14 Example 3 is matched with Comparative Example 1 and the current density is 1000 mA g -1 From the comparison chart of the diaphragm after being disassembled after 300 cycles, it can be seen that under fast charging, the unmodified Na metal negative electrode will quickly consume the electrolyte, and the electrolyte will decompose quickly, resulting in rapid capacity decay; the negative electrode after modifying the Na metal with Bi can solve this problem well and improve its cycle stability.
[0065] Fig.15 The current density of the full battery matched with Prussian blue in Example 4 and Comparative Example 1 is 100 mAg -1 From the comparison of the first cycle charge and discharge curves, it can be seen that the alloying interface formed by Sn metal powder and Na metal can alleviate the voltage drop phenomenon during the discharge process.
[0066] Fig.16The current density of the full cell after matching the Prussian blue of Example 4 and Comparative Example 1 is 100 mA g -1 From the comparison chart after 500 cycles, it can be seen that the capacity of the sodium metal negative electrode without an alloy interface drops rapidly after the electrolyte is consumed after about 450 cycles, while the cycle life is longer when the Sn metal powder and Na metal form an alloy interface.
[0067] Fig.17 The current density of the full battery matched with Prussian blue in Example 5 and Comparative Example 1 is 100 mAg -1 From the comparison of the first cycle charge and discharge curves, it can be seen that the alloying interface formed by Sn metal compound SnF2 powder and Na metal can alleviate the voltage drop phenomenon during the discharge process.
[0068] The above disclosure is only the preferred embodiment of the present invention, which cannot be used to limit the scope of the present invention. Therefore, equivalent changes made according to the claims of the present invention are still within the scope of the present invention.
Claims
1. A process for constructing a sodium-philic alloying interface, characterized in that: The method comprises the following steps: S1, smoothing bulk sodium metal in a glove box, and rolling the bulk sodium metal into smooth and thin sodium metal flakes using a rolling machine; S2, uniformly rolling one or any two of metal powders including Zn, Bi, Sn, Fe, Cu, Ti, Mg, and metal compound powders including SnF2, SnCl3, SnBr3, BiF3, BiCl3, and BiBr3 onto the sodium metal flakes.
2. A process for constructing a sodium-philic alloying interface according to claim 1, characterized in that: The thickness of the sodium metal flakes is 250 um.
3. A process for constructing a sodium-philic alloying interface according to claim 1, characterized in that: The mass percentage of the metal powder or metal compound powder is 1%.
4. A process for constructing a sodium-philic alloying interface according to claim 1, characterized in that: The thickness of the sodium metal alloy composite electrode for constructing the sodium-philic alloying interface is 200 um.
5. A process for constructing a sodium-philic alloying interface according to claim 1, characterized in that: The rolling time is 20-30 minutes.
6. A process for constructing a sodium-philic alloying interface according to claim 1, characterized in that: The protective gas of the glove box is argon or nitrogen.
7. A process for constructing a sodium-philic alloying interface according to claim 1, characterized in that: After rolling evenly, the sodium metal flakes were cut into discs with a diameter of 12 mm.
8. A sodium metal battery prepared by the process for constructing a sodium-philic alloying interface according to any one of claims 1 to 7, characterized in that: It includes positive electrode materials, sodium-philic alloying interface, sodium metal negative electrode and sodium salt organic electrolyte.
9. A sodium metal battery prepared by the process for constructing a sodium-philic alloying interface according to claim 7, characterized in that: In the electrolyte in which the sodium salt solvent is dissolved in the organic solvent, the sodium salt is sodium perchlorate and the solvent is propylene carbonate.
Citation Information
Patent Citations
Sodium metal negative electrode, preparation method thereof and sodium battery
CN116864623A
High-entropy sodium alloy negative electrode, preparation method and sodium battery
CN118448585A
Sodium metal negative electrode containing BiF3 / Na artificial interface layer, preparation method of sodium metal negative electrode and sodium metal battery
CN118553856A
Cited By
Sodium metal negative electrode structure, preparation method thereof and sodium ion battery
CN120149330A