Electrically regulated catalyst and application thereof
Through the use of electrically regulated catalysts, electrochemical stimulation regulates the coordination bonds between Lewis acids and bases, the problem of difficult control of the reaction rate in group transfer polymerization is solved, and the fine regulation of the polymerization reaction and the improvement of product selectivity is achieved.
Patent Information
- Application Number
- CN202411172199.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-12-03
AI Technical Summary
The controllable polymer method for group transfer polymerization has poor fine regulation capabilities during the polymerization process, and the reaction rate is difficult to regulate in real time.
Using an electrical regulation catalyst, Lewis acid combines with Lewis base with electrochemical redox reversibility, and electrochemical stimulation is used to regulate the formation and fracture of its coordination bonds, real-time fine regulation of the polymerization reaction is achieved.
Real-time fine and controllable adjustment of the polymerization reaction process is achieved, and the reaction rate is flexibly controlled, which improves the performance and product selectivity of the polymer.
Smart Images

Figure CN119061433A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer compound synthesis, and in particular to an electrically regulated catalyst and application thereof. Background Art
[0002] Polymer materials are widely used in all walks of life due to their excellent comprehensive performance and the advantages of being light and easy to process. With the advancement of scientific and technological life, people have put forward higher and higher requirements for the performance of polymer materials. The microstructure of a material determines its performance. The controllable synthesis of polymer materials with determined microstructures is a powerful method to improve the performance of polymer materials. Controllable polymerization has the characteristics of preset molecular weight, adjustable molecular weight distribution, and strong design of configuration, and is widely used in the synthesis of functional polymers. According to the polymerization mechanism, controlled polymerization can be divided into three categories: controlled free radical polymerization, controlled ion polymerization, and group transfer polymerization. Among them, group transfer polymerization does not have a polymerization reaction that stops the polymerization chain growth reaction or irreversible side reactions, has stable reaction intermediates, and its catalyst is an organic catalyst with less toxicity. It is widely used in the preparation of active polymers with narrow molecular weight distribution and block copolymers. However, the activity of these organic catalysts is often affected by reaction conditions, such as temperature, solvent, catalyst concentration, etc., so the reaction rate is difficult to control in real time. Therefore, the controllable polymer method based on group transfer polymerization has poor ability to finely control the polymerization process. Summary of the invention
[0003] The problem solved by the present invention is that the controllable polymer method based on group transfer polymerization has poor ability to finely control the polymerization process.
[0004] In order to solve the above problems, the present invention provides an electrically regulated catalyst and application thereof.
[0005] In a first aspect, the present invention provides an electrically regulated catalyst, comprising: a Lewis acid and a Lewis base, wherein the Lewis base is composed of a first active group having electrochemical redox reversibility and a second active group exhibiting Lewis basicity, the first active group and the second active group are bonded to each other via a covalent bond, and the second active group and the Lewis acid are used to form a coordination bond when no electrical stimulation is applied, and the coordination bond is broken or generated when electrical stimulation is applied.
[0006] Optionally, the first active group includes a portion having electrochemical redox reversibility from any one of p-phenylenediamine derivatives, p-benzoquinone derivatives, ferrocene derivatives and tetramethylpiperidinyl oxide derivatives.
[0007] Optionally, the second active group includes a Lewis basic portion from any one of thiophene derivatives, pyridine derivatives, phosphorus-embedded polycyclic aromatic hydrocarbons and oxygen-embedded polycyclic aromatic hydrocarbons.
[0008] Optionally, the first reactive group is derived from a phenylenediamine derivative, and the second reactive group is derived from a pyridine derivative.
[0009] Optionally, the Lewis base has the structural formula:
[0010]
[0011] Wherein, R1, R2, and R3 are H, halogen, C1-C 24 Alkyl, C1-C 24 Substituted alkyl, hydroxyl, C1-C 24 Alkoxy, amino and C1-C 24 Any one of the alkylamino groups.
[0012] Optionally, the molar ratio of the Lewis acid to the Lewis acid base is 1:1-1:10.
[0013] Optionally, the Lewis acid comprises tris(pentafluoro)phenylborane.
[0014] In a second aspect, the present invention provides a use of the electrically regulated catalyst as described above in the preparation of a polymer.
[0015] Optionally, the method of preparing the polymer comprises:
[0016] Dissolving an acrylate monomer, an electrolyte, an initiator, and the electrical regulation catalyst according to any one of claims 1 to 7 in an organic solvent to obtain a mixed solution;
[0017] The mixed solution is placed in an electrochemical reaction cell to carry out a polymerization reaction to obtain a polymer.
[0018] Optionally, the acrylic acid ester monomers include methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, methyl hexyl acrylate, ethyl hexyl acrylate, propyl hexyl acrylate, butyl hexyl acrylate, pentyl hexyl acrylate, hexyl hexyl acrylate, heptyl hexyl acrylate, octyl hexyl acrylate, propyl methyl acrylate, propyl ethyl acrylate, propyl acrylate, propyl butyl acrylate, pentyl acrylate, hexyl propyl acrylate, heptyl propyl acrylate, octyl propyl acrylate, methyl butyl acrylate, ethyl butyl acrylate, propyl butyl acrylate, butyl butyl acrylate, pentyl butyl acrylate, hexyl butyl acrylate, heptyl butyl acrylate, octyl butyl acrylate, methyl pentyl acrylate, ethyl pentyl acrylate, propyl pentyl acrylate, butyl pentyl acrylate, pentyl acrylate, hexyl pentyl acrylate, heptyl pentyl acrylate, octyl butyl acrylate, methyl pentyl acrylate, ethyl pentyl acrylate, propyl pentyl acrylate, butyl pentyl acrylate, pentyl acrylate, hexyl pentyl acrylate, heptyl pentyl acrylate, octyl pentyl acrylate, Octyl acrylate, methyl hexyl acrylate, ethyl hexyl acrylate, propyl hexyl acrylate, butyl hexyl acrylate, pentyl hexyl acrylate, hexyl acrylate, heptyl hexyl acrylate, octyl hexyl acrylate, methyl heptyl acrylate, ethyl heptyl acrylate, propyl heptyl acrylate, butyl heptyl acrylate, pentyl heptyl acrylate, hexyl heptyl acrylate, heptyl heptyl acrylate, octyl heptyl acrylate, methyl octyl acrylate, ethyl octyl acrylate, propyl heptyl acrylate, butyl heptyl acrylate, At least one of octyl pentyl acrylate, octyl hexyl acrylate, octyl heptyl acrylate, octyl octyl acrylate, methyl nonyl acrylate, ethyl nonyl acrylate, propyl nonyl acrylate, butyl nonyl acrylate, pentyl nonyl acrylate, hexyl nonyl acrylate, heptyl nonyl acrylate, octyl nonyl acrylate, methyl decyl acrylate, ethyl decyl acrylate, propyl decyl acrylate, butyl decyl acrylate, pentyl decyl acrylate, hexyl decyl acrylate, heptyl decyl acrylate and octyl decyl acrylate;
[0019] and / or, the electrolyte comprises at least one of tetrabutylammonium hexafluorophosphate, tetrabutylammonium tetrafluoroborate, tetrabutylammonium chloride, tetrabutylammonium iodide, tetrabutylammonium bromide, tetrabutylammonium tribromide, tetrahexylammonium hexafluorophosphate, tetrahexylammonium tetrafluoroborate, tetrahexylammonium chloride, tetrahexylammonium iodide, tetrahexylammonium bromide and tetrahexylammonium tribromide;
[0020] And / or, the initiator includes at least one of dimethylphenylsilyl hydride and dimethylethylsilyl hydride;
[0021] And / or, the organic solvent includes at least one of dichloromethane, chloroform and 1,2-dichloroethane.
[0022] The beneficial effects of the electric control catalyst of the present invention are:
[0023] The electrically regulated catalyst of the present invention combines a portion having electrochemical redox activity with an active portion exhibiting Lewis alkalinity through a covalent bond to obtain an electrochemically regulated Lewis base having electrochemical redox regulation capability and reversibly regulated Lewis alkalinity, that is, the Lewis base changes in alkalinity before and after electrochemical stimulation. Thus, the formation and breaking of the coordination bond between the Lewis base and the Lewis acid can be regulated by changing the electrochemical conditions, such as whether to apply electrical stimulation and the direction of application, thereby adjusting the existence form of the catalyst in the polymerization reaction in real time to achieve real-time fine and controllable regulation of the polymerization reaction process, and this method can control the reaction rate more flexibly. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a flow chart of a method for preparing a polymer in an embodiment of the present invention;
[0025] Figure 2 Schematic diagram of the mechanism of electrochemically regulated non-metallic dynamic coordination bond formation and breaking in an embodiment of the present invention;
[0026] Figure 3 is a schematic diagram of an electrochemical reaction device in an embodiment of the present invention;
[0027] Figure 4 Schematic diagram of the mechanism of fine-tuning the polymerization process by electrochemical stimulation in an embodiment of the present invention;
[0028] Figure 5 The redox property of the Lewis base electrically regulated in Example 1 of the present invention;
[0029] Figure 6 This is the nuclear magnetic structure diagram of the electrically regulated Lewis base and tri(pentafluorophenyl)borane in Example 1 of the present invention;
[0030] Figure 7 The NMR structures of the reaction system under different stimulation voltages in Example 1 of the present invention;
[0031] Figure 8 is the relationship between the conversion rate of the electropolymerized monomer and the reaction time in Example 1 of the present invention;
[0032] Fig. 9 is the relationship between the electropolymerization monomer conversion rate and the reaction time in Example 2 of the present invention;
[0033] Fig.10 is the relationship between the conversion rate of the electropolymerized monomer and the reaction time in Example 3 of the present invention;
[0034] Description of reference numerals:
[0035] 1. Working electrode; 2. Reference electrode; 3. Counter electrode. DETAILED DESCRIPTION
[0036] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.
[0037] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;
[0038] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.
[0039] An embodiment of the present invention provides an electrically regulated catalyst, comprising: a Lewis acid and a Lewis base, wherein the Lewis base is composed of a first active group having electrochemical redox reversibility and a second active group exhibiting Lewis basicity, the first active group and the second active group are bonded to each other via a covalent bond, and the second active group and the Lewis acid are used to form a coordination bond when no electrical stimulation is applied, and the coordination bond is broken or generated when electrical stimulation is applied.
[0040] First of all, it should be noted that in organic chemistry, molecules or atomic groups that can absorb electron clouds are called Lewis acids, and conversely, molecules or atomic groups that can provide electron clouds are called Lewis bases. Lewis bases, or electron donors, are bases defined under the acid-base electronic theory, and refer to molecules or ions that can provide electron pairs. For Lewis bases, since they are usually unsaturated structures (containing non-covalently bonded elements, such as nitrogen, oxygen, sulfur, etc.) and contain highly electronegative atoms, the electron cloud density of the Lewis base with Lewis basicity is relatively large, so that it has the ability to provide electron pairs, can form coordination bonds with Lewis acids, and realize electron transfer in chemical reactions.
[0041] In this embodiment, the electrochemical redox active part and the Lewis basic part with large electron cloud density are combined through covalent bonds to achieve regulation of the molecular electron cloud density.
[0042] Specifically, under the condition that no electrical stimulation is applied, the electrochemically active part (first active group) in the Lewis base does not undergo redox reaction, and the electron cloud density of the part (second active group) in the Lewis base having Lewis basic properties is relatively large, so the second active group in the Lewis base and the Lewis acid are coordinated due to the Lewis acid-base addition reaction to form a complex. It can be understood that the acidity of the Lewis acid has catalytic ability, but when the Lewis acid and the Lewis base coordinate to form a coordination bond, the acidity is suppressed, and the Lewis acid that originally had a catalytic effect loses its catalytic activity due to participation in the coordination reaction, which will affect the progress of the polymerization reaction, which is specifically manifested as a decrease in the rate of the polymerization reaction.
[0043] Under the condition of applying electrical stimulation, the electrochemically active part of the Lewis base undergoes an oxidation reaction, resulting in an overall decrease in the electron cloud density of the Lewis base part, weakening the coordination effect with the Lewis acid, and causing the coordination bond to break. As a result, the acidic part of the decoordinated Lewis acid plays a role and has catalytic activity, thereby catalyzing the polymerization reaction.
[0044] It should be understood that, since the first active group in the Lewis base has electrical redox reversibility, therefore, the process of applying electrical stimulation to break the second active group in the Lewis base and the Lewis acid coordination bond has a reversible recovery ability under the opposite electrical stimulation. That is, when the reverse electrical stimulation is applied, the electron cloud density of the Lewis base returns to the initial state, the coordination bond is regenerated, the acidity of the catalyst Lewis acid is suppressed, and the polymerization reaction rate slows down or even stops. Thus, when the electrical control catalyst of the present embodiment is used for polymerization reaction, the polymerization rate of the polymerization process can be finely controlled in real time by applying positive and negative voltages to the reaction system.
[0045] In this embodiment, the part with electrochemical redox activity is covalently bonded to the active part showing Lewis alkalinity to obtain an electrochemically regulated Lewis base with reversible regulation of Lewis alkalinity with electrochemical redox regulation ability, and the difference in alkalinity of the Lewis base before and after electrochemical stimulation is used. It can be understood that electrochemical stimulation generally refers to the process of inducing electrochemical reactions or changing the behavior of substances under electric fields by applying voltage or current, which is commonly used to control reaction rates, change reaction paths, regulate catalyst activity, etc., and electrochemical stimulation can be achieved by changing electrode potential, current density or applying different electric field conditions. That is, by changing the electrochemical conditions to adjust the properties of the Lewis base, adjust the formation and breakage of the coordination bond between it and the Lewis acid, and then adjust the existence form of the catalyst in the polymerization reaction in real time, so as to achieve real-time fine controllable regulation of the polymerization reaction process, and this method can more flexibly control the reaction rate and product selectivity, providing a new idea for the precise control of the polymerization reaction.
[0046] Optionally, the Lewis acid comprises tri(pentafluoro)phenylborane. The chemical structural formula of tri(pentafluoro)phenylborane is:
[0047]
[0048] Tri(pentafluoro)phenylborane as a Lewis acid catalyst can improve the efficiency and selectivity of the reaction and can be applied to various organic reactions. Therefore, this optional embodiment preferably uses it as the Lewis acid.
[0049] Optionally, the first active group includes a portion having electrochemical redox reversibility from any one of p-phenylenediamine derivatives, p-benzoquinone derivatives, ferrocene derivatives and tetramethylpiperidinyl oxide derivatives.
[0050] In this optional embodiment, the Lewis base is a molecule whose molecular structure and electron cloud density can reversibly change significantly before and after electrochemical stimulation, and is formed by any combination of electrochemically active groups and active parts that exhibit Lewis basicity. Among them, the electrochemically active groups are derived from but not limited to compounds with excellent electrochemical redox reversibility such as p-phenylenediamine derivatives, p-benzoquinone derivatives, ferrocene derivatives, and tetramethylpiperidinyl oxide derivatives. The common chemical groups or structural features in these compounds make them have good reversibility in the electrochemical redox process. For example, the aromatic ring in the p-phenylenediamine derivative has good stability and electron transport performance, so it often shows good reversibility in the electrochemical redox process; p-benzoquinone has an oxygen-containing six-membered ring structure, and the redox reaction of the quinone group can usually occur at different potentials, and its reduction to products such as p-benzoquinone alcohol or aminophenol also has obvious reversibility; ferrocene is a stable iron-ferrocene system, and iron redox reactions usually occur in the electrochemical process, and these reactions have good reversibility; tetramethylpiperidin oxide derivatives are a class of oxygen-containing heterocyclic compounds, in which oxygen atoms are easy to accept or release electrons, so the redox reaction between them and the reducing agent usually also shows good reversibility. Therefore, the present embodiment selects the groups or molecular structures in these compounds as the first active groups.
[0051] Optionally, the second active group includes a Lewis basic portion from any one of thiophene derivatives, pyridine derivatives, phosphorus-embedded polycyclic aromatic hydrocarbons and oxygen-embedded polycyclic aromatic hydrocarbons.
[0052] In this optional embodiment, compounds with high electron cloud density such as thiophene derivatives, pyridine derivatives, phosphorus-embedded polycyclic aromatic hydrocarbons, oxygen-embedded polycyclic aromatic hydrocarbons, etc. are selected as the alkaline active part of the Lewis base. This is mainly because the electron rings (such as π bonds, lone pairs of electrons, etc.) inside these compounds with large electron cloud density are more likely to provide electrons. Therefore, when reacting with Lewis acids, these compounds are more likely to exhibit the properties of Lewis bases.
[0053] The Lewis base can be obtained by combining the first active group and the second active group in any way and combining the two parts by covalent bonds. It should be understood that the above examples are not exhaustive, and only some preferred examples are listed, as long as the first active group and the second active group each have the conditions of electrochemical activity and Lewis basicity.
[0054] Optionally, the first reactive group is derived from a phenylenediamine derivative, and the second reactive group is derived from a pyridine derivative.
[0055] In this optional embodiment, a p-phenylenediamine derivative is used as the electrochemical redox part, and a pyridine derivative is used as the Lewis base part, and the two parts are combined by covalent bonds to obtain an electrically regulated Lewis base. Among them, p-phenylenediamine derivatives are a class of compounds with good electrochemical activity, which are easy to undergo redox reactions in electrochemical processes. By introducing different functional groups into the p-phenylenediamine structure, its electron cloud density and the position of the redox peak can be regulated, so as an electrochemical redox part, a variety of adjustable properties can be provided. Pyridine derivatives usually have good Lewis base properties and can effectively donate lone pairs of electrons to Lewis acids. By combining p-phenylenediamine derivatives and pyridine derivatives by covalent bonds, the interaction between the two can be enhanced, the stability of the electrically regulated Lewis base can be improved, and by regulating the structure and ratio of the two parts, the electrochemical activity of the electrically regulated Lewis base, the properties of the Lewis base, etc. can be precisely controlled.
[0056] Optionally, the Lewis base has the structural formula:
[0057]
[0058] Wherein, R1, R2, and R3 are H, halogen, C1-C 24 Alkyl, C1-C 24 Substituted alkyl, hydroxyl, C1-C 24 Alkoxy, amino and C1-C 24 Any one of the alkylamino groups.
[0059] In this optional embodiment, a p-phenylenediamine derivative is selected as the electrochemical redox part, a pyridine derivative is selected as the Lewis base part, and a Lewis base having the above-mentioned structural formula is obtained by covalent bonding. This helps to bring out the respective advantages of the two parts, improve the performance and stability of the composite, and also has controllability and adjustability. That is, the electrochemical redox active part and the Lewis base part with high electron cloud density are bonded by covalent bonds using a CN coupling reaction, thereby achieving regulation of the molecular electron cloud density, and preparing for the subsequent preparation of an electrically regulated catalyst in a polymerization reaction.
[0060] Optionally, the molar ratio of the Lewis acid to the Lewis acid base is 1:1-1:10.
[0061] Keeping the molar ratio of Lewis acid to Lewis base in the range of 1:1-1:10 helps to make full use of the interaction between Lewis acid and Lewis base and obtain efficient catalytic activity under specific conditions. Such a molar ratio range can ensure the formation of a reasonable complex or intermediate between the acid and the base, thereby promoting the progress of a specific chemical reaction. In addition, in the Lewis acid-base reaction, the molar ratio of Lewis acid to Lewis base will affect the progress of the chemical reaction. The molar ratio in the above range can control the selectivity of the product, thereby achieving effective control of the reaction process, while preventing unreacted Lewis acid or Lewis base from becoming a product or initiating a side reaction, which helps to improve the purity and yield of the target product.
[0062] An embodiment of the present invention provides an application of the electrically regulated catalyst as described in any one of the above items in the preparation of a polymer.
[0063] Since electrically regulated catalysts can adjust the properties of Lewis bases according to electrochemical stimulation, causing the formation or breaking of coordination bonds between them and Lewis acids, their use in the polymer preparation process is beneficial for real-time regulation of the presence form of the catalyst in the polymerization reaction, thereby achieving real-time, finely controllable regulation of the polymerization reaction process.
[0064] Optionally, see Figure 1 As shown, the method for preparing the polymer comprises:
[0065] Dissolving an acrylate monomer, an electrolyte, an initiator, and the electrical regulation catalyst described in any one of the above items in an organic solvent to obtain a mixed solution;
[0066] The mixed solution is placed in an electrochemical reaction cell to carry out a polymerization reaction to obtain a polymer.
[0067] Optionally, the step of placing the mixed solution into an electrochemical reaction cell to perform a polymerization reaction to obtain a polymer comprises:
[0068] An inert electrode with stable electrochemical properties is used as a working electrode and a counter electrode, and a silver electrode is used as a reference electrode. Polymerization is carried out at room temperature under anhydrous and oxygen-free conditions, the reaction is quenched, and the reaction solution is sunk in a poor solvent to obtain a polymer.
[0069] The purpose of sinking the reaction liquid into a poor solvent is to precipitate or coagulate the polymer so that it can be separated from the reaction liquid. By adding the reaction liquid mixture into the poor solvent, the compatibility between the poor solvent and the polymer is low, resulting in precipitation or coagulation of the polymer, thereby obtaining a relatively pure polymer product.
[0070] Optionally, the acrylic acid ester monomers include methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, methyl hexyl acrylate, ethyl hexyl acrylate, propyl hexyl acrylate, butyl hexyl acrylate, pentyl hexyl acrylate, hexyl hexyl acrylate, heptyl hexyl acrylate, octyl hexyl acrylate, propyl methyl acrylate, propyl ethyl acrylate, propyl acrylate, propyl butyl acrylate, pentyl acrylate, hexyl propyl acrylate, heptyl propyl acrylate, octyl propyl acrylate, methyl butyl acrylate, ethyl butyl acrylate, propyl butyl acrylate, butyl butyl acrylate, pentyl butyl acrylate, hexyl butyl acrylate, heptyl butyl acrylate, octyl butyl acrylate, methyl pentyl acrylate, ethyl pentyl acrylate, propyl pentyl acrylate, butyl pentyl acrylate, pentyl acrylate, hexyl pentyl acrylate, heptyl pentyl acrylate, octyl butyl acrylate, methyl pentyl acrylate, ethyl pentyl acrylate, propyl pentyl acrylate, butyl pentyl acrylate, pentyl acrylate, hexyl pentyl acrylate, heptyl pentyl acrylate, octyl pentyl acrylate, Octyl acrylate, methyl hexyl acrylate, ethyl hexyl acrylate, propyl hexyl acrylate, butyl hexyl acrylate, pentyl hexyl acrylate, hexyl acrylate, heptyl hexyl acrylate, octyl hexyl acrylate, methyl heptyl acrylate, ethyl heptyl acrylate, propyl heptyl acrylate, butyl heptyl acrylate, pentyl heptyl acrylate, hexyl heptyl acrylate, heptyl heptyl acrylate, octyl heptyl acrylate, methyl octyl acrylate, ethyl octyl acrylate, propyl heptyl acrylate, butyl heptyl acrylate, At least one of octyl pentyl acrylate, octyl hexyl acrylate, octyl heptyl acrylate, octyl octyl acrylate, methyl nonyl acrylate, ethyl nonyl acrylate, propyl nonyl acrylate, butyl nonyl acrylate, pentyl nonyl acrylate, hexyl nonyl acrylate, heptyl nonyl acrylate, octyl nonyl acrylate, methyl decyl acrylate, ethyl decyl acrylate, propyl decyl acrylate, butyl decyl acrylate, pentyl decyl acrylate, hexyl decyl acrylate, heptyl decyl acrylate and octyl decyl acrylate.
[0071] In this optional embodiment, the acrylic acid ester monomers include various group structures such as methyl, hexyl, propyl, pentyl, hexyl, heptyl, octyl, nonyl and decyl, and different monomers can be selected when synthesizing polymers to achieve regulation of polymer structure and performance. In addition, these acrylic acid ester monomers have good reactivity, are easy to undergo free radical polymerization, and generally have a faster reaction rate during the polymerization reaction, which is conducive to improving the efficiency of the polymerization reaction.
[0072] Optionally, the electrolyte includes at least one of tetrabutylammonium hexafluorophosphate, tetrabutylammonium tetrafluoroborate, tetrabutylammonium chloride, tetrabutylammonium iodide, tetrabutylammonium bromide, tetrabutylammonium tribromide, tetrahexylammonium hexafluorophosphate, tetrahexylammonium tetrafluoroborate, tetrahexylammonium chloride, tetrahexylammonium iodide, tetrahexylammonium bromide and tetrahexylammonium tribromide.
[0073] This optional embodiment selects tetraalkyl ammonium salt as electrolyte, and tetraalkyl ammonium salt can be dissociated into positively charged ions in organic solvents, which is conducive to increasing the specific conductivity of the reaction system, improving the diffusion rate of the electrolyte in the reaction, thereby promoting the transmission of the electrolyte and the carrying out of the reaction. And the structure of tetraalkyl ammonium salt is stable, not easy to decompose, and can maintain good stability in the electrochemical reaction process, which helps to maintain the stability of the reaction system and avoids the adverse effects of the electrolyte. Therefore, selecting tetraalkyl ammonium salt as electrolyte helps to realize the efficient carrying out of electrochemical reaction and the accurate control of polymerization process.
[0074] Optionally, the initiator includes at least one of dimethylphenylsilyl hydride and dimethylethylsilyl hydride.
[0075] Dimethylphenylsilyl hydride and dimethylethylsilyl hydride are commonly used silicon hydride compounds. They can quickly release free groups when initiating polymerization reactions, effectively initiate the polymerization reaction of monomers, and have good initiation effects. In addition, these two initiators have good solubility, are easy to prepare and operate, and are convenient for control and adjustment in experiments, which is conducive to achieving precise control of the polymerization reaction process.
[0076] Optionally, the organic solvent includes at least one of dichloromethane, chloroform and 1,2-dichloroethane.
[0077] In this optional embodiment, organic solvents such as dichloromethane, chloroform and 1,2-dichloroethane generally have good solubility, which helps to dissolve the reaction materials and products therein, forming a uniform reaction system, which is beneficial to the progress and control of the reaction.
[0078] The following is an explanation of the regulation and control mechanism of the polymerization reaction by the electrically regulated catalyst in the embodiment of the present invention, taking the structure in which the Lewis acid is (pentafluoro)phenylborane represented by formula (1) and the Lewis base is represented by formula (2) as an example.
[0079] See also Figure 2 The figure shows the mechanism of electrochemically regulated non-metallic dynamic coordination bonds. When no electrical stimulation is applied, tri(pentafluorophenyl)borane with Lewis acidity and Lewis base with Lewis basicity coordinate to form a complex due to Lewis acid-base addition. After electrochemical stimulation is applied, the electrochemically active part of the Lewis base undergoes oxidation reaction, and the overall electron cloud of the molecule is conjugated to the pyridine part that mainly exhibits Lewis basicity, so that its electron cloud density is reduced, thereby causing the non-metallic coordination bond to break. The whole process has reversible recovery ability under the opposite electrical stimulation.
[0080] In the process of preparing the polymer, the electrically regulated catalyst is used to regulate the polymerization process based on electrically regulated non-metallic dynamic coordination bonds. The polymerization method with finely regulated polymerization process includes:
[0081] The electrically regulated catalyst is prepared by dissolving tri(pentafluorophenyl)borane having strong Lewis acidity and an electrically regulated Lewis base in a non-polar protic solvent;
[0082] dissolving an acrylate monomer, an initiator, and an electrolyte in an aprotic solvent;
[0083] The solution containing the electric regulating catalyst is slowly added dropwise to the solution containing the monomer, initiator, and electrolyte, and then transferred to the electrochemical reaction cell. The device structure is as follows: Figure 3 As shown, in the electrochemical reaction, a platinum mesh is used as a working electrode 1, a platinum wire is used as a counter electrode 3, and a silver wire is used as a reference electrode 2, and a polymerization reaction is carried out under magnetic stirring.
[0084] A constant voltage direct current is applied to the system to regulate the reaction process.
[0085] Among them, the mechanism of electrochemical stimulation fine-tuning the polymerization process is as follows Figure 4 As shown, specifically, in Figure 2 The electrochemical reversible regulation of the formation and breaking of nonmetallic dynamic coordination bonds is based on the strong Lewis acidity of sp 2 The catalytic ability of the hybridized tri(pentafluorophenyl)borane is that when no electrical stimulation is initially applied, tri(pentafluorophenyl)borane coordinates with the pyridine part of the electrically regulated Lewis base (to distinguish it from the conventional Lewis base, it is referred to as the electrically regulated Lewis base, the same below), causing its Lewis acidity to decrease and it has no catalytic ability. After applying electrical stimulation, the electrically induced Lewis base is oxidized, the electron cloud density decreases, and the coordination bond breaks. The strong Lewis acidity of tri(pentafluorophenyl)borane comes into play again, catalyzing the polymerization of the reaction. At the same time, under the stimulation of reverse voltage, the electron cloud density of the electrically regulated Lewis base returns to the initial state, the coordination bond is regenerated, the acidity of the catalyst is suppressed, and the polymerization reaction rate slows down or even stops. Based on the above process, the polymerization rate of the polymerization process can be finely controlled in real time by applying positive and reverse voltages to the system.
[0086] Therefore, by designing an electrically regulated catalyst composed of an electrically regulated Lewis base and tri(pentafluorophenyl)borane, and utilizing the changes in Lewis acidity before and after electrical stimulation, real-time regulation of the reaction rate of the polymerization process is achieved, laying the foundation for more precise customization of polymer materials and the realization of polymers with specific functions.
[0087] The present invention is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on the conditions recommended by the manufacturer.
[0088] Example 1
[0089] In this embodiment, the electrochemically controllable polymerization system is composed of formula (2-1) as an electrically adjustable Lewis base, tri(pentafluorophenyl)borane as an acid-adjustable catalyst, methyl methacrylate as a polymerization monomer, dimethylphenylsilane as an initiator, tetrabutylammonium iodide as an electrolyte, and dichloromethane as a solvent. Wherein formula (2-1) is formula (2) wherein R1 is hydrogen, and R2 and R3 are methyl groups.
[0090]
[0091] Among them, the electrochemical redox properties of the Lewis base represented by formula (2-1) are as follows Figure 5 shown.
[0092] according to Figure 5 It can be seen that with the application of positive voltage, two oxidation peaks appear in succession in the electrically-regulated Lewis base, corresponding to the two-step electrochemical oxidation reaction of the electrically-regulated Lewis base. At the same time, under the voltage stimulation in the opposite direction, the corresponding electrochemical reduction peak appears, proving that the electrically-regulated Lewis base has good electrochemical redox reversibility.
[0093] The coordination interaction between the electrically regulated Lewis base and tri(pentafluorophenyl)borane was confirmed by NMR characterization, such as Figure 6 As shown, Figure 6 (a) is the nuclear magnetic resonance spectrum after the electrically regulated Lewis base is coordinated with tri(pentafluorophenyl)borane. Figure 6 (b) is the NMR spectrum of the electrically regulated Lewis base. It can be seen that with the addition of electron-deficient tri(pentafluorophenyl)borane, the characteristic hydrogen of the electrically regulated Lewis base moves to the low field region (as shown in the figure by Figure 6 (b) To Figure 6 (arrow shown in (a)), which proves the occurrence of Lewis acid-base coordination.
[0094] In the process of preparing the polymer, the polymerization process based on the electrically regulated non-metallic dynamic coordination bond is regulated, and the steps are as follows:
[0095] 1.1. Dissolve 240 mg of tri(pentafluorophenyl)borane and 100 mg of electrically regulated Lewis base (Formula (2-1)) in anhydrous and oxygen-free dichloromethane solvent, stir and dissolve to obtain a uniformly mixed solution, which is an electrically regulated catalyst solution;
[0096] 1.2. Dissolve 315 mg of methyl methacrylate, 10.4 mg of tetrabutylammonium iodide, and 17 mg of dimethylphenylsilane in anhydrous and oxygen-free dichloromethane solvent;
[0097] 1.3. Slowly drop the solution containing the electric regulation catalyst into the solution containing the acrylic ester monomer;
[0098] 1.4. Using platinum mesh as working electrode, platinum wire as counter electrode and silver wire as reference electrode, apply 0 V voltage to the electropolymerization system for 1 h;
[0099] 1.5. Apply +1.2V voltage to the electropolymerization system for 2h;
[0100] 1.6. Apply a voltage of -0.6 V to the electropolymerization system for 2 h.
[0101] The electrically controlled polymerization process of this embodiment can be characterized by NMR, such as Figure 7 As shown, the reaction solution at different reaction times was characterized by NMR, and then, Figure 7 The arrow a in the middle represents the characteristic hydrogen of the acrylate monomer (hereinafter referred to as the monomer), and the arrow b represents the characteristic hydrogen of the polymer generated by the polymerization reaction. The monomer conversion rate of the reaction is obtained by comparing the area of the characteristic hydrogen of the polymer with the total area of the characteristic hydrogen of the monomer and the polymer.
[0102] The monomer conversion rate changes with time. Figure 8 As shown. Figure 8 It can be seen that when no voltage is initially applied to the electropolymerization system (0V), tri(pentafluoro)phenylborane coordinates with the electrically regulated Lewis base, has no catalytic activity, and the polymerization reaction does not occur; when a positive voltage stimulus is applied to the system (+1.2V), the electrochemically active part of the electrically regulated Lewis base undergoes an oxidation reaction, and its electron cloud density decreases as a whole, and it decoordinates with tri(pentafluoro)phenylborane, and the released tri(pentafluoro)phenylborane has catalytic activity, and the catalytic reaction proceeds; when a reverse voltage is applied to the system (-0.6V), the electrically regulated Lewis base is reduced to the initial state of high electron cloud density, and again coordinates with tri(pentafluorophenyl)borane, loses its catalytic activity, and reduces the polymerization reaction rate.
[0103] Example 2
[0104] The difference between this embodiment and embodiment 1 is that the structural formula of the electrically regulated Lewis acid is different, and the voltage applied to the electropolymerization system is slightly different.
[0105] In this embodiment, the electrochemically controllable polymerization system is composed of formula (2-2) as an electrically adjustable Lewis base, tri(pentafluorophenyl)borane as an acidic adjustable catalyst, methyl methacrylate as a polymerization monomer, dimethylphenylsilane as an initiator, tetrabutylammonium iodide as an electrolyte, and dichloromethane as a solvent. The formula (2-2) is that R1 in formula (2) is N,N-dimethylphenyl, and R2 and R3 are methyl groups.
[0106]
[0107] In the process of preparing the polymer, the polymerization process based on the electrically regulated non-metallic dynamic coordination bond is regulated, and the steps are as follows:
[0108] 2.1. Dissolve 240 mg of tri(pentafluorophenyl)borane and 100 mg of electrically regulated Lewis base in anhydrous and oxygen-free dichloromethane solvent, stir and dissolve to obtain a uniformly mixed solution, which is an electrically regulated catalyst solution;
[0109] 2.2. Dissolve 315 mg of methyl methacrylate, 10.4 mg of tetrabutylammonium iodide, and 17 mg of dimethylphenylsilane in anhydrous and oxygen-free dichloromethane solvent;
[0110] 2.3. Slowly drop the solution containing the electrical regulation catalyst into the solution containing the monomer;
[0111] 2.4. Using platinum mesh as working electrode, platinum wire as counter electrode and silver wire as reference electrode, apply 0 V voltage to the electropolymerization system for 1 h;
[0112] 2.5. Apply a voltage of +1.3 V to the electropolymerization system for 2 h;
[0113] 2.6. Apply a voltage of -0.7 V to the electropolymerization system for 2 h.
[0114] In this embodiment, the conversion rate of the monomers was obtained after NMR characterization of the electrically controlled polymerization process. The trend of the monomer conversion rate over time is shown in Fig. 9 As shown, the overall trend is similar to that of Example 1. When no electrical stimulation is applied (corresponding to the 0V stage in the figure), the polymerization reaction does not occur; when a forward electrical stimulation is applied (corresponding to the +1.3V stage in the figure), the polymerization reaction proceeds; when a reverse electrical stimulation is applied (corresponding to the -0.7V stage in the figure), the polymerization reaction rate decreases.
[0115] Example 3
[0116] The difference between this embodiment and embodiment 1 is that the type and amount of the acrylic acid ester monomer are different.
[0117] In this embodiment, the electrochemically controllable polymerization system is composed of formula (2-1) as an electrically adjustable Lewis base, tri(pentafluorophenyl)borane as an acidic adjustable catalyst, butyl methacrylate as a polymerization monomer, dimethylphenylsilane as an initiator, tetrabutylammonium iodide as an electrolyte, and dichloromethane as a solvent.
[0118] In the process of preparing the polymer, the polymerization process based on the electrically regulated non-metallic dynamic coordination bond is regulated, and the steps are as follows:
[0119] 3.1. Dissolve 240 mg of tri(pentafluorophenyl)borane and 400 mg of electrically regulated Lewis base in anhydrous and oxygen-free dichloromethane solvent, stir and dissolve to obtain a uniformly mixed solution, which is an electrically regulated catalyst solution;
[0120] 3.2. Dissolve 448 mg of butyl methacrylate, 10.4 mg of tetrabutylammonium iodide, and 17 mg of dimethylphenylsilane in anhydrous and oxygen-free dichloromethane solvent;
[0121] 3.3. Slowly drop the solution containing the electrical regulation catalyst into the solution containing the monomer;
[0122] 3.4. Using platinum mesh as working electrode, platinum wire as counter electrode and silver wire as reference electrode, apply 0 V voltage to the electropolymerization system for 1 h;
[0123] 3.5. Apply a voltage of +1.2 V to the electropolymerization system for 2 h;
[0124] 3.6. Apply a voltage of -0.6 V to the electropolymerization system for 2 h.
[0125] In this embodiment, the conversion rate of the monomers was obtained after NMR characterization of the electrically controlled polymerization process. The trend of the monomer conversion rate over time is shown in Fig.10 As shown, the overall trend is similar to that of Example 1 and will not be repeated here.
[0126] Example 4
[0127] The difference between this embodiment and embodiment 1 is that the electrolyte is different.
[0128] In this embodiment, the electrochemically controllable polymerization system is composed of formula (2-1) as an electrically adjustable Lewis base, tri(pentafluorophenyl)borane as an acidic adjustable catalyst, methyl methacrylate as a polymerization monomer, dimethylphenylsilane as an initiator, tetrabutylammonium bromide as an electrolyte, and dichloromethane as a solvent.
[0129] In the process of preparing the polymer, the polymerization process based on the electrically regulated non-metallic dynamic coordination bond is regulated, and the steps are as follows:
[0130] 4.1. Dissolve 240 mg of tri(pentafluorophenyl)borane and 100 mg of electrically regulated Lewis base in anhydrous and oxygen-free dichloromethane solvent, stir and dissolve to obtain a uniformly mixed solution, which is an electrically regulated catalyst solution;
[0131] 4.2. Dissolve 315 mg of methyl methacrylate, 10.4 mg of tetrabutylammonium bromide, and 17 mg of dimethylphenylsilane in anhydrous and oxygen-free dichloromethane solvent;
[0132] 4.3. Slowly drop the solution containing the electrical regulation catalyst into the solution containing the monomer;
[0133] 4.4. Using platinum mesh as working electrode, platinum wire as counter electrode and silver wire as reference electrode, apply 0 V voltage to the electropolymerization system for 1 h;
[0134] 4.5. Apply a voltage of +1.2 V to the electropolymerization system for 2 h;
[0135] 4.6. Apply a voltage of -0.6 V to the electropolymerization system for 2 h.
[0136] Example 5
[0137] The difference between this embodiment and embodiment 1 is that the Lewis base structure is different.
[0138] In this embodiment, the electrochemically controllable polymerization system is composed of formula (2-3) as an electrically adjustable Lewis base, tri(pentafluorophenyl)borane as an acid-adjustable catalyst, methyl methacrylate as a polymerization monomer, dimethylphenylsilane as an initiator, tetrabutylammonium iodide as an electrolyte, and dichloromethane as a solvent. Wherein formula (2-3) is that R1, R2, and R3 in formula (2) are methyl groups.
[0139]
[0140] In the process of preparing the polymer, the polymerization process based on the electrically regulated non-metallic dynamic coordination bond is regulated, and the steps are as follows:
[0141] 5.1. Dissolve 240 mg of tri(pentafluorophenyl)borane and 100 mg of electrically regulated Lewis base in anhydrous and oxygen-free dichloromethane solvent, stir and dissolve to obtain a uniformly mixed solution, which is an electrically regulated catalyst solution;
[0142] 5.2. Dissolve 315 mg of methyl methacrylate, 10.4 mg of tetrabutylammonium iodide, and 17 mg of dimethylphenylsilane in anhydrous and oxygen-free dichloromethane solvent;
[0143] 5.3. Slowly drop the solution containing the electrical regulation catalyst into the solution containing the monomer;
[0144] 5.4. Using platinum mesh as working electrode, platinum wire as counter electrode and silver wire as reference electrode, apply 0 V voltage to the electropolymerization system for 1 h;
[0145] 5.5. Apply a voltage of +1.3 V to the electropolymerization system for 2 h;
[0146] 5.6. Apply a voltage of -0.7 V to the electropolymerization system for 2 h.
[0147] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.
Claims
1. An electrically regulated catalyst, characterized in that: include: A Lewis acid and a Lewis base, wherein the Lewis base is composed of a first active group having electrochemical redox reversibility and a second active group exhibiting Lewis alkalinity, the first active group and the second active group are bonded via a covalent bond, the second active group is used to form a coordination bond with the Lewis acid when no electrical stimulation is applied, and the coordination bond is broken or generated when electrical stimulation is applied.
2. The electrically regulated catalyst according to claim 1, characterized in that , wherein the first active group includes a portion having electrochemical redox reversibility from any one of a p-phenylenediamine derivative, a p-benzoquinone derivative, a ferrocene derivative and a tetramethylpiperidinyl oxide derivative.
3. The electrically controlled catalyst according to claim 1, characterized in that: The second active group includes a part having Lewis basicity from any one of thiophene derivatives, pyridine derivatives, phosphorus-embedded polycyclic aromatic hydrocarbons and oxygen-embedded polycyclic aromatic hydrocarbons.
4. The electrically regulated catalyst according to claim 1, characterized in that ,, the first active group comes from a phenylenediamine derivative, and the second active group comes from a pyridine derivative.
5. The electrically regulated catalyst according to claim 1, characterized in that ,, the structural formula of the Lewis base is: Wherein, R1, R2, and R3 are H, halogen, C1-C 24 Alkyl, C1-C 24 Substituted alkyl, hydroxyl, C1-C 24 Alkoxy, amino and C1-C 24 Any one of the alkylamino groups.
6. The electrically regulated catalyst according to claim 1, characterized in that ,, the molar ratio of the Lewis acid to the Lewis acid base is 1:1-1:
10.
7. The electrically regulated catalyst according to claim 1, characterized in that ,, the Lewis acid includes tri(pentafluoro)phenylborane.
8. Use of the electrically regulated catalyst according to any one of claims 1 to 7 in the preparation of polymers.
9. The use according to claim 8, characterized in that: The method for preparing a polymer comprises: Dissolving an acrylate monomer, an electrolyte, an initiator, and the electrical regulation catalyst according to any one of claims 1 to 7 in an organic solvent to obtain a mixed solution; The mixed solution is placed in an electrochemical reaction cell to carry out a polymerization reaction to obtain a polymer.
10. The use according to claim 9, characterized in that: The acrylic ester monomers include methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, pentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, methyl hexyl acrylate, ethyl hexyl acrylate, propyl hexyl acrylate, butyl hexyl acrylate, pentyl hexyl acrylate, hexyl hexyl acrylate, heptyl hexyl acrylate, octyl hexyl acrylate, propyl methyl acrylate, propyl ethyl acrylate, propyl acrylate, propyl butyl acrylate, pentyl propyl acrylate, hexyl propyl acrylate, heptyl propyl acrylate, octyl propyl acrylate, methyl butyl acrylate, ethyl butyl acrylate, propyl butyl acrylate, butyl butyl acrylate, pentyl butyl acrylate, hexyl butyl acrylate, heptyl butyl acrylate, octyl butyl acrylate, methyl pentyl acrylate, ethyl pentyl acrylate, propyl pentyl acrylate, butyl pentyl acrylate, pentyl butyl acrylate, hexyl butyl acrylate, heptyl butyl acrylate, octyl butyl acrylate, methyl pentyl acrylate, ethyl pentyl acrylate, propyl pentyl acrylate, butyl pentyl acrylate, pentyl pentyl acrylate, hexyl pentyl acrylate, heptyl pentyl acrylate, octyl pentyl acrylate, Octyl acrylate, hexyl methyl acrylate, hexyl ethyl acrylate, hexyl propyl acrylate, hexyl butyl acrylate, hexyl pentyl acrylate, hexyl acrylate, heptyl acrylate, heptyl octyl acrylate, heptyl methyl acrylate, heptyl ethyl acrylate, heptyl propyl acrylate, heptyl butyl acrylate, heptyl pentyl acrylate, heptyl heptyl acrylate, heptyl heptyl acrylate, heptyl octyl acrylate, octyl methyl acrylate, octyl ethyl acrylate, octyl propyl acrylate, octyl butyl acrylate, octyl at least one of pentyl acrylate, octyl hexyl acrylate, octyl heptyl acrylate, octyl octyl acrylate, methyl nonyl acrylate, ethyl nonyl acrylate, propyl nonyl acrylate, butyl nonyl acrylate, pentyl nonyl acrylate, hexyl nonyl acrylate, heptyl nonyl acrylate, octyl nonyl acrylate, methyl decyl acrylate, ethyl decyl acrylate, propyl decyl acrylate, butyl decyl acrylate, pentyl decyl acrylate, hexyl decyl acrylate, heptyl decyl acrylate and octyl decyl acrylate; and / or, the electrolyte comprises at least one of tetrabutylammonium hexafluorophosphate, tetrabutylammonium tetrafluoroborate, tetrabutylammonium chloride, tetrabutylammonium iodide, tetrabutylammonium bromide, tetrabutylammonium tribromide, tetrahexylammonium hexafluorophosphate, tetrahexylammonium tetrafluoroborate, tetrahexylammonium chloride, tetrahexylammonium iodide, tetrahexylammonium bromide and tetrahexylammonium tribromide; And / or, the initiator includes at least one of dimethylphenylsilyl hydride and dimethylethylsilyl hydride; And / or, the organic solvent includes at least one of dichloromethane, chloroform and 1,2-dichloroethane.